- Verification
- /
- Failure
Composite failure criteria against lab tests
First-ply and progressive failure predictions compared with failure loads measured on coupons and tubes, and with published answers.
How close the results are
Lab tests show how close a prediction comes to a measured part. Reference solutions show that the program solves its equations the way someone else solved the same problem. A case is one configuration checked against one source, and it scores by its value with the largest error. A lab case that runs every failure criterion or every micromechanics model scores by Puck (the Puck failure criterion or the Puck micromechanics model), the same choice for all of them. The other models show in its row. Fitted cases show in their source but stay out of every number.
Lab tests: strength
Validation: failure loads of coupons, tubes, beams and joints, compared with published test programs. Where the app has several failure criteria, a case scores by Puck. The other criteria show in its row.
- Cases
- 146 cases from 4 sources, 1314 compared numbers
- Within 10 %
- 64 of 146
- Median error
- 7.91 %, known gaps left out
- Bias and scatter
- −1.45 % on average, ±10.2 % scatter (1 SD)
- Known gaps
- 42, see the list
Published solutions
Verification: the same inputs run against worked examples, tables and closed-form answers printed in textbooks, NASA reports and journal papers.
- Cases
- 4 cases from 1 source, 26 compared numbers
- Within 1 %
- 4 of 4
- Median error
- <0.001 %
- Largest error
- <0.001 %
- Known gaps
- None
Finite element models
Verification: a plane-stress finite element model of the same problem, solved in an open-source code. Each model runs on two meshes.
No finite element model is listed for failure yet.
ABD Composites runs no tests of its own. Each measured value comes from a published test program.
Sources
Each row is one source the results are checked against. Error is the difference between the program's value and the source's value, as a percentage of the source's value. A reference case passes at 1 % or less, a lab case at 10 % or less. Open a row to see every case, its chart and how to reproduce each number.
Soden, P. D., Hinton, M. J. & Kaddour, A. S., Biaxial Test Results for Strength and Deformation of a Range of E-Glass and Carbon Fibre Reinforced Composite Laminates: Failure Exercise Benchmark Data, Compos. Sci. Technol. 62 (2002) 1489-1514. Lamina properties from Soden, Hinton & Kaddour, Compos. Sci. Technol. 58 (1998) 1011-1022, Table 1.
Measured [MPa]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41 failure stress magnitude [MPa], PuckWhy: The paper reports this tube as a suspected buckling or grip failure, which a failure criterion does not model. At least one criterion falls outside the band. | 407.71 | 1010.5 | +147.9 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42 failure stress magnitude [MPa], PuckWhy: The paper reports this tube as a suspected buckling or grip failure, which a failure criterion does not model. At least one criterion falls outside the band. | 382.79 | 809.49 | +111.5 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43 failure stress magnitude [MPa], PuckWhy: The paper reports this tube as a suspected buckling or grip failure, which a failure criterion does not model. At least one criterion falls outside the band. | 386.77 | 807.29 | +108.7 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39 failure stress magnitude [MPa], PuckWhy: The paper reports this tube as a suspected buckling or grip failure, which a failure criterion does not model. At least one criterion falls outside the band. | 516.86 | 941.68 | +82.2 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 305.82 | 548.03 | +79.2 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 328.4 | 548.03 | +66.9 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 329 | 548.03 | +66.6 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 324.5 | 499.81 | +54.0 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 359.69 | 535.06 | +48.8 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 368.43 | 548.03 | +48.7 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 442.05 | 634.91 | +43.6 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 393.06 | 548.03 | +39.4 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 404 | 548.03 | +35.7 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 470.25 | 631.19 | +34.2 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 420.56 | 560.59 | +33.3 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 733 | 548.03 | −25.2 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 782.14 | 633.01 | −19.1 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 421.9 | 498.13 | +18.1 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 504.77 | 594 | +17.7 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 761 | 650.92 | −14.5 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 640 | 548.03 | −14.4 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 752 | 650.92 | −13.4 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1038.5 | 912.2 | −12.2 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 808.55 | 717.39 | −11.3 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 564.73 | 626.67 | +11.0 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1212 | 1084.6 | −10.5 % | Over 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 958.6 | 872.07 | −9.03 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 722.94 | 662.86 | −8.31 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 947.06 | 872.03 | −7.92 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 718.89 | 661.95 | −7.92 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 725.05 | 668.37 | −7.82 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 711.94 | 766.46 | +7.66 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 960.89 | 893.53 | −7.01 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 814.61 | 768.13 | −5.71 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 677.84 | 656.59 | −3.14 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 925.38 | 903.6 | −2.35 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40 failure stress magnitude [MPa], PuckWhy: The paper reports this tube as a suspected buckling or grip failure, which a failure criterion does not model. At least one criterion falls outside the band. | 665.69 | 680.49 | +2.22 % | Known gap |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32 failure stress magnitude [MPa], Puck | 537 | 548.03 | +2.05 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 757.91 | 742.87 | −1.99 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 707.1 | 700.18 | −0.98 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 645.47 | 642.7 | −0.43 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 668.65 | 667.05 | −0.24 % | Within 10 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 652 | 650.92 | −0.17 % | Within 10 % |
How to reproduce it
Source
Soden, P. D., Hinton, M. J. & Kaddour, A. S., Biaxial Test Results for Strength and Deformation of a Range of E-Glass and Carbon Fibre Reinforced Composite Laminates: Failure Exercise Benchmark Data, Compos. Sci. Technol. 62 (2002) 1489-1514. Lamina properties from Soden, Hinton & Kaddour, Compos. Sci. Technol. 58 (1998) 1011-1022, Table 1.
Table 9
What was taken from it
The measured axial and hoop failure stresses of the [90/±45/0]s tubes, every test set the table prints.
Quantity compared: failure stress magnitude [MPa]
Inputs
- Laminate [90/45/-45/0/0/-45/45/90] of AS4/3501-6. The load grows along the measured σ<sub>x</sub> to σ<sub>y</sub> ratio until the progressive failure tool reaches last-ply failure.
- Compared value: the failure stress magnitude along that ratio, MPa.
- The paper marks some tubes under axial compression and external pressure as suspected buckling or grip failures. They are listed, and a failure criterion does not model either mode.
- Every failure criterion the app has is a sub-case of each test, run with the app's default parameters. Nothing is tuned to the test and no cure residual stress is applied.
- The lamina strengths are the exercise's benchmark inputs. Soden et al. (1998) call them typical values derived by a variety of methods, so they are not the strengths of the tubes that were tested.
The inputs of each configuration are listed in the table below.
Allowed difference
±20 %; outside it, known gap
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41, Tsai-Wu | quasi-isotropic | 407.71 | 1644.1 | +303.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42, Tsai-Wu | quasi-isotropic | 382.79 | 1304.1 | +240.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43, Tsai-Wu | quasi-isotropic | 386.77 | 1298.2 | +235.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39, Tsai-Wu | quasi-isotropic | 516.86 | 1477.9 | +185.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41, Max Strain | quasi-isotropic | 407.71 | 1107.3 | +171.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41, Max Stress | quasi-isotropic | 407.71 | 1077.4 | +164.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41, Hashin | quasi-isotropic | 407.71 | 1077.4 | +164.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41, Sun | quasi-isotropic | 407.71 | 1077.4 | +164.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41, Puck | quasi-isotropic | 407.71 | 1010.5 | +147.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41, Edge | quasi-isotropic | 407.71 | 1004.6 | +146.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41, Cuntze (FMC) | quasi-isotropic | 407.71 | 933.64 | +129.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 41, Tsai-Hill | quasi-isotropic | 407.71 | 906.34 | +122.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42, Max Strain | quasi-isotropic | 382.79 | 821.46 | +114.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43, Max Strain | quasi-isotropic | 386.77 | 819.13 | +111.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42, Max Stress | quasi-isotropic | 382.79 | 809.49 | +111.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42, Hashin | quasi-isotropic | 382.79 | 809.49 | +111.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42, Puck | quasi-isotropic | 382.79 | 809.49 | +111.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42, Sun | quasi-isotropic | 382.79 | 809.49 | +111.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43, Max Stress | quasi-isotropic | 386.77 | 807.29 | +108.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43, Hashin | quasi-isotropic | 386.77 | 807.29 | +108.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43, Puck | quasi-isotropic | 386.77 | 807.29 | +108.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43, Sun | quasi-isotropic | 386.77 | 807.29 | +108.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42, Cuntze (FMC) | quasi-isotropic | 382.79 | 781.49 | +104.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43, Cuntze (FMC) | quasi-isotropic | 386.77 | 779.88 | +101.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42, Tsai-Hill | quasi-isotropic | 382.79 | 762.69 | +99.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43, Tsai-Hill | quasi-isotropic | 386.77 | 760.17 | +96.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1, Cuntze (FMC) | quasi-isotropic | 305.82 | 599.9 | +96.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1, Tsai-Wu | quasi-isotropic | 305.82 | 587.45 | +92.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2, Cuntze (FMC) | quasi-isotropic | 328.4 | 599.9 | +82.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38, Cuntze (FMC) | quasi-isotropic | 329 | 599.9 | +82.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39, Puck | quasi-isotropic | 516.86 | 941.68 | +82.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39, Max Strain | quasi-isotropic | 516.86 | 941.16 | +82.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1, Sun | quasi-isotropic | 305.82 | 549.3 | +79.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1, Puck | quasi-isotropic | 305.82 | 548.03 | +79.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2, Tsai-Wu | quasi-isotropic | 328.4 | 587.45 | +78.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38, Tsai-Wu | quasi-isotropic | 329 | 587.45 | +78.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39, Max Stress | quasi-isotropic | 516.86 | 922.25 | +78.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39, Hashin | quasi-isotropic | 516.86 | 922.25 | +78.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39, Sun | quasi-isotropic | 516.86 | 922.25 | +78.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30, Tsai-Hill | quasi-isotropic | 1212 | 301.5 | −75.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29, Tsai-Hill | quasi-isotropic | 1038.5 | 276.76 | −73.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30, Tsai-Wu | quasi-isotropic | 1212 | 332.32 | −72.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27, Tsai-Hill | quasi-isotropic | 960.89 | 273.93 | −71.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15, Tsai-Hill | quasi-isotropic | 958.6 | 279.11 | −70.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16, Tsai-Hill | quasi-isotropic | 947.06 | 279.13 | −70.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29, Tsai-Wu | quasi-isotropic | 1038.5 | 306.23 | −70.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1, Max Stress | quasi-isotropic | 305.82 | 520.92 | +70.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1, Hashin | quasi-isotropic | 305.82 | 520.92 | +70.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28, Tsai-Hill | quasi-isotropic | 925.38 | 275.46 | −70.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1, Max Strain | quasi-isotropic | 305.82 | 520.09 | +70.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27, Tsai-Wu | quasi-isotropic | 960.89 | 311.97 | −67.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2, Sun | quasi-isotropic | 328.4 | 549.3 | +67.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38, Sun | quasi-isotropic | 329 | 549.3 | +67.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2, Puck | quasi-isotropic | 328.4 | 548.03 | +66.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15, Tsai-Wu | quasi-isotropic | 958.6 | 318.34 | −66.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28, Tsai-Wu | quasi-isotropic | 925.38 | 308.88 | −66.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38, Puck | quasi-isotropic | 329 | 548.03 | +66.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16, Tsai-Wu | quasi-isotropic | 947.06 | 318.36 | −66.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39, Cuntze (FMC) | quasi-isotropic | 516.86 | 855.85 | +65.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3, Cuntze (FMC) | quasi-isotropic | 368.43 | 599.9 | +62.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39, Tsai-Hill | quasi-isotropic | 516.86 | 838.36 | +62.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13, Tsai-Wu | quasi-isotropic | 782.14 | 299.72 | −61.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26, Tsai-Hill | quasi-isotropic | 814.61 | 315.06 | −61.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12, Tsai-Wu | quasi-isotropic | 564.73 | 221.37 | −60.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17, Tsai-Wu | quasi-isotropic | 722.94 | 283.96 | −60.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23, Tsai-Wu | quasi-isotropic | 718.89 | 283.1 | −60.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22, Tsai-Wu | quasi-isotropic | 808.55 | 320.12 | −60.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25, Tsai-Wu | quasi-isotropic | 725.05 | 288.99 | −60.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22, Tsai-Hill | quasi-isotropic | 808.55 | 325.28 | −59.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3, Tsai-Wu | quasi-isotropic | 368.43 | 587.45 | +59.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 42, Edge | quasi-isotropic | 382.79 | 609.49 | +59.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26, Tsai-Wu | quasi-isotropic | 814.61 | 333.52 | −59.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13, Tsai-Hill | quasi-isotropic | 782.14 | 322.8 | −58.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2, Max Stress | quasi-isotropic | 328.4 | 520.92 | +58.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2, Hashin | quasi-isotropic | 328.4 | 520.92 | +58.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2, Max Strain | quasi-isotropic | 328.4 | 520.09 | +58.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38, Max Stress | quasi-isotropic | 329 | 520.92 | +58.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38, Hashin | quasi-isotropic | 329 | 520.92 | +58.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38, Max Strain | quasi-isotropic | 329 | 520.09 | +58.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17, Tsai-Hill | quasi-isotropic | 722.94 | 305.52 | −57.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23, Tsai-Hill | quasi-isotropic | 718.89 | 304.65 | −57.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19, Tsai-Hill | quasi-isotropic | 757.91 | 321.92 | −57.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25, Tsai-Hill | quasi-isotropic | 725.05 | 310.29 | −57.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21, Tsai-Wu | quasi-isotropic | 668.65 | 287.82 | −57.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 43, Edge | quasi-isotropic | 386.77 | 606.76 | +56.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19, Tsai-Wu | quasi-isotropic | 757.91 | 329.16 | −56.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24, Tsai-Wu | quasi-isotropic | 707.1 | 312.48 | −55.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18, Tsai-Hill | quasi-isotropic | 711.94 | 315.58 | −55.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12, Tsai-Hill | quasi-isotropic | 564.73 | 251.64 | −55.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24, Tsai-Hill | quasi-isotropic | 707.1 | 324.44 | −54.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5, Max Stress | quasi-isotropic | 324.5 | 499.81 | +54.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5, Hashin | quasi-isotropic | 324.5 | 499.81 | +54.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5, Puck | quasi-isotropic | 324.5 | 499.81 | +54.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5, Sun | quasi-isotropic | 324.5 | 499.81 | +54.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5, Cuntze (FMC) | quasi-isotropic | 324.5 | 499.81 | +54.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5, Max Strain | quasi-isotropic | 324.5 | 499.81 | +54.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11, Tsai-Wu | quasi-isotropic | 504.77 | 232.97 | −53.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21, Tsai-Hill | quasi-isotropic | 668.65 | 309.22 | −53.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18, Tsai-Wu | quasi-isotropic | 711.94 | 333.36 | −53.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4, Cuntze (FMC) | quasi-isotropic | 393.06 | 599.9 | +52.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10, Tsai-Wu | quasi-isotropic | 470.25 | 227.27 | −51.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20, Tsai-Hill | quasi-isotropic | 677.84 | 332.53 | −50.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4, Tsai-Wu | quasi-isotropic | 393.06 | 587.45 | +49.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1, Edge | quasi-isotropic | 305.82 | 456.69 | +49.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9, Tsai-Wu | quasi-isotropic | 442.05 | 224.46 | −49.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3, Sun | quasi-isotropic | 368.43 | 549.3 | +49.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7, Max Stress | quasi-isotropic | 359.69 | 535.06 | +48.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7, Hashin | quasi-isotropic | 359.69 | 535.06 | +48.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7, Puck | quasi-isotropic | 359.69 | 535.06 | +48.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7, Sun | quasi-isotropic | 359.69 | 535.06 | +48.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7, Cuntze (FMC) | quasi-isotropic | 359.69 | 535.06 | +48.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7, Max Strain | quasi-isotropic | 359.69 | 535.06 | +48.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3, Puck | quasi-isotropic | 368.43 | 548.03 | +48.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37, Cuntze (FMC) | quasi-isotropic | 404 | 599.9 | +48.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 39, Edge | quasi-isotropic | 516.86 | 759.24 | +46.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 1, Tsai-Hill | quasi-isotropic | 305.82 | 445.53 | +45.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11, Tsai-Hill | quasi-isotropic | 504.77 | 274.23 | −45.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37, Tsai-Wu | quasi-isotropic | 404 | 587.45 | +45.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10, Tsai-Hill | quasi-isotropic | 470.25 | 263.98 | −43.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20, Tsai-Wu | quasi-isotropic | 677.84 | 380.89 | −43.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9, Max Stress | quasi-isotropic | 442.05 | 634.91 | +43.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9, Hashin | quasi-isotropic | 442.05 | 634.91 | +43.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9, Puck | quasi-isotropic | 442.05 | 634.91 | +43.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9, Sun | quasi-isotropic | 442.05 | 634.91 | +43.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9, Edge | quasi-isotropic | 442.05 | 634.91 | +43.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8, Tsai-Wu | quasi-isotropic | 420.56 | 241.73 | −42.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9, Max Strain | quasi-isotropic | 442.05 | 628 | +42.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9, Tsai-Hill | quasi-isotropic | 442.05 | 258.48 | −41.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3, Max Stress | quasi-isotropic | 368.43 | 520.92 | +41.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3, Hashin | quasi-isotropic | 368.43 | 520.92 | +41.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3, Max Strain | quasi-isotropic | 368.43 | 520.09 | +41.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4, Sun | quasi-isotropic | 393.06 | 549.3 | +39.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4, Puck | quasi-isotropic | 393.06 | 548.03 | +39.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31, Tsai-Hill | quasi-isotropic | 733 | 445.53 | −39.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2, Edge | quasi-isotropic | 328.4 | 456.69 | +39.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38, Edge | quasi-isotropic | 329 | 456.69 | +38.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 9, Cuntze (FMC) | quasi-isotropic | 442.05 | 613.2 | +38.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31, Edge | quasi-isotropic | 733 | 456.69 | −37.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37, Sun | quasi-isotropic | 404 | 549.3 | +36.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35, Tsai-Hill | quasi-isotropic | 761 | 487.5 | −35.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35, Tsai-Wu | quasi-isotropic | 761 | 487.5 | −35.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 2, Tsai-Hill | quasi-isotropic | 328.4 | 445.53 | +35.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37, Puck | quasi-isotropic | 404 | 548.03 | +35.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 38, Tsai-Hill | quasi-isotropic | 329 | 445.53 | +35.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36, Tsai-Hill | quasi-isotropic | 752 | 487.5 | −35.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36, Tsai-Wu | quasi-isotropic | 752 | 487.5 | −35.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40, Tsai-Wu | quasi-isotropic | 665.69 | 898.15 | +34.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10, Max Stress | quasi-isotropic | 470.25 | 631.19 | +34.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10, Hashin | quasi-isotropic | 470.25 | 631.19 | +34.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10, Puck | quasi-isotropic | 470.25 | 631.19 | +34.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10, Sun | quasi-isotropic | 470.25 | 631.19 | +34.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10, Edge | quasi-isotropic | 470.25 | 631.19 | +34.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10, Max Strain | quasi-isotropic | 470.25 | 631.19 | +34.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8, Max Stress | quasi-isotropic | 420.56 | 560.59 | +33.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8, Hashin | quasi-isotropic | 420.56 | 560.59 | +33.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8, Puck | quasi-isotropic | 420.56 | 560.59 | +33.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8, Sun | quasi-isotropic | 420.56 | 560.59 | +33.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8, Edge | quasi-isotropic | 420.56 | 560.59 | +33.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8, Cuntze (FMC) | quasi-isotropic | 420.56 | 560.59 | +33.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8, Max Strain | quasi-isotropic | 420.56 | 560.59 | +33.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4, Max Stress | quasi-isotropic | 393.06 | 520.92 | +32.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4, Hashin | quasi-isotropic | 393.06 | 520.92 | +32.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4, Max Strain | quasi-isotropic | 393.06 | 520.09 | +32.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14, Tsai-Wu | quasi-isotropic | 645.47 | 438.6 | −32.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14, Tsai-Hill | quasi-isotropic | 645.47 | 439.42 | −31.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 8, Tsai-Hill | quasi-isotropic | 420.56 | 288.88 | −31.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 10, Cuntze (FMC) | quasi-isotropic | 470.25 | 615.58 | +30.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33, Tsai-Hill | quasi-isotropic | 640 | 445.53 | −30.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7, Tsai-Wu | quasi-isotropic | 359.69 | 253.33 | −29.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40, Edge | quasi-isotropic | 665.69 | 471.74 | −29.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6, Tsai-Wu | quasi-isotropic | 421.9 | 299.33 | −29.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31, Max Strain | quasi-isotropic | 733 | 520.09 | −29.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37, Max Stress | quasi-isotropic | 404 | 520.92 | +28.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37, Hashin | quasi-isotropic | 404 | 520.92 | +28.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31, Max Stress | quasi-isotropic | 733 | 520.92 | −28.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31, Hashin | quasi-isotropic | 733 | 520.92 | −28.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37, Max Strain | quasi-isotropic | 404 | 520.09 | +28.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33, Edge | quasi-isotropic | 640 | 456.69 | −28.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26, Cuntze (FMC) | quasi-isotropic | 814.61 | 601.77 | −26.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31, Puck | quasi-isotropic | 733 | 548.03 | −25.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34, Tsai-Hill | quasi-isotropic | 652 | 487.5 | −25.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34, Tsai-Wu | quasi-isotropic | 652 | 487.5 | −25.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31, Sun | quasi-isotropic | 733 | 549.3 | −25.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3, Edge | quasi-isotropic | 368.43 | 456.69 | +24.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6, Edge | quasi-isotropic | 421.9 | 321.53 | −23.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 3, Tsai-Hill | quasi-isotropic | 368.43 | 445.53 | +20.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31, Tsai-Wu | quasi-isotropic | 733 | 587.45 | −19.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13, Max Strain | quasi-isotropic | 782.14 | 630.81 | −19.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13, Cuntze (FMC) | quasi-isotropic | 782.14 | 631.71 | −19.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13, Max Stress | quasi-isotropic | 782.14 | 633.01 | −19.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13, Hashin | quasi-isotropic | 782.14 | 633.01 | −19.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13, Puck | quasi-isotropic | 782.14 | 633.01 | −19.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13, Sun | quasi-isotropic | 782.14 | 633.01 | −19.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 13, Edge | quasi-isotropic | 782.14 | 633.01 | −19.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33, Max Strain | quasi-isotropic | 640 | 520.09 | −18.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33, Max Stress | quasi-isotropic | 640 | 520.92 | −18.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33, Hashin | quasi-isotropic | 640 | 520.92 | −18.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 31, Cuntze (FMC) | quasi-isotropic | 733 | 599.9 | −18.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6, Max Stress | quasi-isotropic | 421.9 | 498.13 | +18.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6, Hashin | quasi-isotropic | 421.9 | 498.13 | +18.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6, Puck | quasi-isotropic | 421.9 | 498.13 | +18.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6, Sun | quasi-isotropic | 421.9 | 498.13 | +18.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6, Cuntze (FMC) | quasi-isotropic | 421.9 | 498.13 | +18.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6, Max Strain | quasi-isotropic | 421.9 | 498.13 | +18.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22, Cuntze (FMC) | quasi-isotropic | 808.55 | 664.74 | −17.8 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11, Max Stress | quasi-isotropic | 504.77 | 594 | +17.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11, Hashin | quasi-isotropic | 504.77 | 594 | +17.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11, Puck | quasi-isotropic | 504.77 | 594 | +17.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11, Sun | quasi-isotropic | 504.77 | 594 | +17.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11, Edge | quasi-isotropic | 504.77 | 594 | +17.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11, Cuntze (FMC) | quasi-isotropic | 504.77 | 594 | +17.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 11, Max Strain | quasi-isotropic | 504.77 | 594 | +17.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 6, Tsai-Hill | quasi-isotropic | 421.9 | 347.4 | −17.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32, Tsai-Hill | quasi-isotropic | 537 | 445.53 | −17.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4, Edge | quasi-isotropic | 393.06 | 456.69 | +16.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19, Cuntze (FMC) | quasi-isotropic | 757.91 | 635.91 | −16.1 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18, Cuntze (FMC) | quasi-isotropic | 711.94 | 604.06 | −15.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32, Edge | quasi-isotropic | 537 | 456.69 | −15.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7, Tsai-Hill | quasi-isotropic | 359.69 | 307.27 | −14.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35, Max Strain | quasi-isotropic | 761 | 650.12 | −14.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35, Cuntze (FMC) | quasi-isotropic | 761 | 650.82 | −14.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35, Max Stress | quasi-isotropic | 761 | 650.92 | −14.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35, Hashin | quasi-isotropic | 761 | 650.92 | −14.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35, Puck | quasi-isotropic | 761 | 650.92 | −14.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35, Sun | quasi-isotropic | 761 | 650.92 | −14.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 35, Edge | quasi-isotropic | 761 | 650.92 | −14.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33, Puck | quasi-isotropic | 640 | 548.03 | −14.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33, Sun | quasi-isotropic | 640 | 549.3 | −14.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36, Max Strain | quasi-isotropic | 752 | 650.12 | −13.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36, Cuntze (FMC) | quasi-isotropic | 752 | 650.82 | −13.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36, Max Stress | quasi-isotropic | 752 | 650.92 | −13.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36, Hashin | quasi-isotropic | 752 | 650.92 | −13.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36, Puck | quasi-isotropic | 752 | 650.92 | −13.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36, Sun | quasi-isotropic | 752 | 650.92 | −13.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 36, Edge | quasi-isotropic | 752 | 650.92 | −13.4 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 4, Tsai-Hill | quasi-isotropic | 393.06 | 445.53 | +13.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37, Edge | quasi-isotropic | 404 | 456.69 | +13.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29, Max Strain | quasi-isotropic | 1038.5 | 910.53 | −12.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29, Cuntze (FMC) | quasi-isotropic | 1038.5 | 912.2 | −12.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29, Max Stress | quasi-isotropic | 1038.5 | 912.2 | −12.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29, Hashin | quasi-isotropic | 1038.5 | 912.2 | −12.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29, Puck | quasi-isotropic | 1038.5 | 912.2 | −12.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29, Sun | quasi-isotropic | 1038.5 | 912.2 | −12.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 29, Edge | quasi-isotropic | 1038.5 | 912.2 | −12.2 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40, Tsai-Hill | quasi-isotropic | 665.69 | 586.4 | −11.9 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32, Cuntze (FMC) | quasi-isotropic | 537 | 599.9 | +11.7 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22, Max Stress | quasi-isotropic | 808.55 | 714.43 | −11.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22, Hashin | quasi-isotropic | 808.55 | 714.43 | −11.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22, Sun | quasi-isotropic | 808.55 | 714.43 | −11.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22, Edge | quasi-isotropic | 808.55 | 714.43 | −11.6 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22, Max Strain | quasi-isotropic | 808.55 | 717.02 | −11.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 22, Puck | quasi-isotropic | 808.55 | 717.39 | −11.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12, Max Stress | quasi-isotropic | 564.73 | 626.67 | +11.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12, Hashin | quasi-isotropic | 564.73 | 626.67 | +11.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12, Puck | quasi-isotropic | 564.73 | 626.67 | +11.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12, Sun | quasi-isotropic | 564.73 | 626.67 | +11.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12, Edge | quasi-isotropic | 564.73 | 626.67 | +11.0 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30, Cuntze (FMC) | quasi-isotropic | 1212 | 1084.6 | −10.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30, Max Stress | quasi-isotropic | 1212 | 1084.6 | −10.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30, Hashin | quasi-isotropic | 1212 | 1084.6 | −10.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30, Puck | quasi-isotropic | 1212 | 1084.6 | −10.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30, Sun | quasi-isotropic | 1212 | 1084.6 | −10.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30, Edge | quasi-isotropic | 1212 | 1084.6 | −10.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 30, Max Strain | quasi-isotropic | 1212 | 1084.6 | −10.5 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 37, Tsai-Hill | quasi-isotropic | 404 | 445.53 | +10.3 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12, Max Strain | quasi-isotropic | 564.73 | 620.79 | +9.93 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32, Tsai-Wu | quasi-isotropic | 537 | 587.45 | +9.39 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5, Tsai-Wu | quasi-isotropic | 324.5 | 294.65 | −9.20 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15, Max Strain | quasi-isotropic | 958.6 | 870.68 | −9.17 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15, Cuntze (FMC) | quasi-isotropic | 958.6 | 872.07 | −9.03 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15, Max Stress | quasi-isotropic | 958.6 | 872.07 | −9.03 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15, Hashin | quasi-isotropic | 958.6 | 872.07 | −9.03 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15, Puck | quasi-isotropic | 958.6 | 872.07 | −9.03 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15, Sun | quasi-isotropic | 958.6 | 872.07 | −9.03 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 15, Edge | quasi-isotropic | 958.6 | 872.07 | −9.03 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17, Max Strain | quasi-isotropic | 722.94 | 662.79 | −8.32 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 12, Cuntze (FMC) | quasi-isotropic | 564.73 | 611.66 | +8.31 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17, Cuntze (FMC) | quasi-isotropic | 722.94 | 662.86 | −8.31 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17, Max Stress | quasi-isotropic | 722.94 | 662.86 | −8.31 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17, Hashin | quasi-isotropic | 722.94 | 662.86 | −8.31 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17, Puck | quasi-isotropic | 722.94 | 662.86 | −8.31 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17, Sun | quasi-isotropic | 722.94 | 662.86 | −8.31 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 17, Edge | quasi-isotropic | 722.94 | 662.86 | −8.31 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33, Tsai-Wu | quasi-isotropic | 640 | 587.45 | −8.21 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16, Max Strain | quasi-isotropic | 947.06 | 870.64 | −8.07 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 7, Edge | quasi-isotropic | 359.69 | 330.92 | −8.00 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23, Max Strain | quasi-isotropic | 718.89 | 661.83 | −7.94 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16, Cuntze (FMC) | quasi-isotropic | 947.06 | 872.03 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16, Max Stress | quasi-isotropic | 947.06 | 872.03 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16, Hashin | quasi-isotropic | 947.06 | 872.03 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16, Puck | quasi-isotropic | 947.06 | 872.03 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16, Sun | quasi-isotropic | 947.06 | 872.03 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 16, Edge | quasi-isotropic | 947.06 | 872.03 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23, Cuntze (FMC) | quasi-isotropic | 718.89 | 661.95 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23, Max Stress | quasi-isotropic | 718.89 | 661.95 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23, Hashin | quasi-isotropic | 718.89 | 661.95 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23, Puck | quasi-isotropic | 718.89 | 661.95 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23, Sun | quasi-isotropic | 718.89 | 661.95 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 23, Edge | quasi-isotropic | 718.89 | 661.95 | −7.92 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25, Cuntze (FMC) | quasi-isotropic | 725.05 | 668.21 | −7.84 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25, Max Stress | quasi-isotropic | 725.05 | 668.37 | −7.82 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25, Hashin | quasi-isotropic | 725.05 | 668.37 | −7.82 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25, Puck | quasi-isotropic | 725.05 | 668.37 | −7.82 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25, Sun | quasi-isotropic | 725.05 | 668.37 | −7.82 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25, Edge | quasi-isotropic | 725.05 | 668.37 | −7.82 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 25, Max Strain | quasi-isotropic | 725.05 | 668.61 | −7.78 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18, Puck | quasi-isotropic | 711.94 | 766.46 | +7.66 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18, Max Strain | quasi-isotropic | 711.94 | 765.77 | +7.56 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27, Max Strain | quasi-isotropic | 960.89 | 891.99 | −7.17 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27, Cuntze (FMC) | quasi-isotropic | 960.89 | 893.53 | −7.01 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27, Max Stress | quasi-isotropic | 960.89 | 893.53 | −7.01 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27, Hashin | quasi-isotropic | 960.89 | 893.53 | −7.01 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27, Puck | quasi-isotropic | 960.89 | 893.53 | −7.01 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27, Sun | quasi-isotropic | 960.89 | 893.53 | −7.01 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 27, Edge | quasi-isotropic | 960.89 | 893.53 | −7.01 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18, Max Stress | quasi-isotropic | 711.94 | 760.99 | +6.89 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18, Hashin | quasi-isotropic | 711.94 | 760.99 | +6.89 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18, Sun | quasi-isotropic | 711.94 | 760.99 | +6.89 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 18, Edge | quasi-isotropic | 711.94 | 760.99 | +6.89 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26, Max Stress | quasi-isotropic | 814.61 | 762.57 | −6.39 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26, Hashin | quasi-isotropic | 814.61 | 762.57 | −6.39 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26, Sun | quasi-isotropic | 814.61 | 762.57 | −6.39 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26, Edge | quasi-isotropic | 814.61 | 762.57 | −6.39 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5, Tsai-Hill | quasi-isotropic | 324.5 | 344.92 | +6.29 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 33, Cuntze (FMC) | quasi-isotropic | 640 | 599.9 | −6.27 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26, Max Strain | quasi-isotropic | 814.61 | 767.43 | −5.79 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 26, Puck | quasi-isotropic | 814.61 | 768.13 | −5.71 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24, Cuntze (FMC) | quasi-isotropic | 707.1 | 675.13 | −4.52 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20, Max Strain | quasi-isotropic | 677.84 | 656.14 | −3.20 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32, Max Strain | quasi-isotropic | 537 | 520.09 | −3.15 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20, Cuntze (FMC) | quasi-isotropic | 677.84 | 656.56 | −3.14 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20, Max Stress | quasi-isotropic | 677.84 | 656.59 | −3.14 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20, Hashin | quasi-isotropic | 677.84 | 656.59 | −3.14 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20, Puck | quasi-isotropic | 677.84 | 656.59 | −3.14 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20, Sun | quasi-isotropic | 677.84 | 656.59 | −3.14 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 20, Edge | quasi-isotropic | 677.84 | 656.59 | −3.14 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32, Max Stress | quasi-isotropic | 537 | 520.92 | −3.00 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32, Hashin | quasi-isotropic | 537 | 520.92 | −3.00 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40, Hashin | quasi-isotropic | 665.69 | 645.96 | −2.96 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40, Max Strain | quasi-isotropic | 665.69 | 685.3 | +2.95 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19, Max Stress | quasi-isotropic | 757.91 | 738.6 | −2.55 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19, Hashin | quasi-isotropic | 757.91 | 738.6 | −2.55 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19, Sun | quasi-isotropic | 757.91 | 738.6 | −2.55 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19, Edge | quasi-isotropic | 757.91 | 738.6 | −2.55 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28, Max Strain | quasi-isotropic | 925.38 | 902 | −2.53 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28, Cuntze (FMC) | quasi-isotropic | 925.38 | 903.6 | −2.35 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28, Max Stress | quasi-isotropic | 925.38 | 903.6 | −2.35 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28, Hashin | quasi-isotropic | 925.38 | 903.6 | −2.35 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28, Puck | quasi-isotropic | 925.38 | 903.6 | −2.35 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28, Sun | quasi-isotropic | 925.38 | 903.6 | −2.35 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 28, Edge | quasi-isotropic | 925.38 | 903.6 | −2.35 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32, Sun | quasi-isotropic | 537 | 549.3 | +2.29 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40, Max Stress | quasi-isotropic | 665.69 | 680.49 | +2.22 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40, Puck | quasi-isotropic | 665.69 | 680.49 | +2.22 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40, Sun | quasi-isotropic | 665.69 | 680.49 | +2.22 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19, Max Strain | quasi-isotropic | 757.91 | 742.33 | −2.06 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 32, Puck | quasi-isotropic | 537 | 548.03 | +2.05 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 19, Puck | quasi-isotropic | 757.91 | 742.87 | −1.99 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 40, Cuntze (FMC) | quasi-isotropic | 665.69 | 676.51 | +1.63 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24, Max Stress | quasi-isotropic | 707.1 | 700.18 | −0.98 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24, Hashin | quasi-isotropic | 707.1 | 700.18 | −0.98 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24, Puck | quasi-isotropic | 707.1 | 700.18 | −0.98 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24, Sun | quasi-isotropic | 707.1 | 700.18 | −0.98 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24, Edge | quasi-isotropic | 707.1 | 700.18 | −0.98 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 5, Edge | quasi-isotropic | 324.5 | 321.58 | −0.90 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 24, Max Strain | quasi-isotropic | 707.1 | 702.08 | −0.71 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14, Max Strain | quasi-isotropic | 645.47 | 641.32 | −0.64 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14, Cuntze (FMC) | quasi-isotropic | 645.47 | 642.31 | −0.49 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14, Max Stress | quasi-isotropic | 645.47 | 642.7 | −0.43 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14, Hashin | quasi-isotropic | 645.47 | 642.7 | −0.43 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14, Puck | quasi-isotropic | 645.47 | 642.7 | −0.43 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14, Sun | quasi-isotropic | 645.47 | 642.7 | −0.43 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 14, Edge | quasi-isotropic | 645.47 | 642.7 | −0.43 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34, Max Strain | quasi-isotropic | 652 | 650.12 | −0.29 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21, Cuntze (FMC) | quasi-isotropic | 668.65 | 666.99 | −0.25 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21, Max Stress | quasi-isotropic | 668.65 | 667.05 | −0.24 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21, Hashin | quasi-isotropic | 668.65 | 667.05 | −0.24 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21, Puck | quasi-isotropic | 668.65 | 667.05 | −0.24 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21, Sun | quasi-isotropic | 668.65 | 667.05 | −0.24 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21, Edge | quasi-isotropic | 668.65 | 667.05 | −0.24 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 21, Max Strain | quasi-isotropic | 668.65 | 667.22 | −0.21 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34, Cuntze (FMC) | quasi-isotropic | 652 | 650.82 | −0.18 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34, Max Stress | quasi-isotropic | 652 | 650.92 | −0.17 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34, Hashin | quasi-isotropic | 652 | 650.92 | −0.17 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34, Puck | quasi-isotropic | 652 | 650.92 | −0.17 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34, Sun | quasi-isotropic | 652 | 650.92 | −0.17 % |
| WWFE-I AS4/3501-6 quasi-isotropic σx-σy, point 34, Edge | quasi-isotropic | 652 | 650.92 | −0.17 % |
Clay, S. B. & Knoth, P. M., "Experimental Results of Quasi-Static Testing for Calibration and Validation of Composite Progressive Damage Analysis Methods", J Compos Mater 51 (2017) 1333-1353.
Measured [MPa]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension unnotched strength [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 473 | 871.5 | +84.2 % | Known gap |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression unnotched strength [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 382 | 566.07 | +48.2 % | Known gap |
| IM7/977-3 [60/0/-60]3S unnotched compression unnotched strength [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 765 | 603.11 | −21.2 % | Known gap |
| IM7/977-3 [0/45/90/-45]2S unnotched tension unnotched strength [MPa], Puck | 866 | 968.56 | +11.8 % | Over 10 % |
| IM7/977-3 [60/0/-60]3S unnotched tension unnotched strength [MPa], Puck | 1005 | 968.56 | −3.63 % | Within 10 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression unnotched strength [MPa], Puck | 603 | 603.11 | +0.019 % | Within 10 % |
How to reproduce it
Source
Clay, S. B. & Knoth, P. M., "Experimental Results of Quasi-Static Testing for Calibration and Validation of Composite Progressive Damage Analysis Methods", J Compos Mater 51 (2017) 1333-1353.
Table 3 (p. 9); ply data Table 2 (p. 6)
What was taken from it
The mean unnotched tension and compression strength of the three layups, with the ply strengths the same program measured.
Quantity compared: unnotched strength [MPa]
Inputs
- IM7/977-3 ply, Table 2: XT 2905, XC 1569, YT 78.9, YC 248 MPa. S12 99.4 MPa is the value at 5 % shear strain, the closest the paper prints to an ultimate.
- Tension layups use the tension moduli and compression layups the compression moduli.
- Uniaxial σ<sub>x</sub>, last-ply failure of the progressive failure tool.
- Every failure criterion the app has is a sub-case of each test, run with the app's default parameters. Nothing is tuned to the test and no cure residual stress is applied.
- The laminates have a lower fiber volume (63.1 %) than the ply panels (68.5 %), which raises a fiber-governed prediction above the test.
The inputs of each configuration are listed in the table below.
Allowed difference
±20 %; outside it, known gap
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension, Max Strain | angle-ply | 473 | 871.5 | +84.2 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension, Max Stress | angle-ply | 473 | 871.5 | +84.2 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension, Puck | angle-ply | 473 | 871.5 | +84.2 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension, Sun | angle-ply | 473 | 871.5 | +84.2 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension, Edge | angle-ply | 473 | 871.5 | +84.2 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension, Cuntze (FMC) | angle-ply | 473 | 871.5 | +84.2 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression, Max Strain | angle-ply | 382 | 609.31 | +59.5 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression, Max Stress | angle-ply | 382 | 605 | +58.4 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression, Sun | angle-ply | 382 | 605 | +58.4 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression, Hashin | angle-ply | 382 | 578.47 | +51.4 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression, Puck | angle-ply | 382 | 566.07 | +48.2 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression, Cuntze (FMC) | angle-ply | 382 | 514.04 | +34.6 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension, Tsai-Wu | angle-ply | 473 | 328.09 | −30.6 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression, Tsai-Wu | angle-ply | 382 | 486.12 | +27.3 % |
| IM7/977-3 [60/0/-60]3S unnotched compression, Cuntze (FMC) | quasi-isotropic | 765 | 603.11 | −21.2 % |
| IM7/977-3 [60/0/-60]3S unnotched compression, Max Stress | quasi-isotropic | 765 | 603.11 | −21.2 % |
| IM7/977-3 [60/0/-60]3S unnotched compression, Hashin | quasi-isotropic | 765 | 603.11 | −21.2 % |
| IM7/977-3 [60/0/-60]3S unnotched compression, Puck | quasi-isotropic | 765 | 603.11 | −21.2 % |
| IM7/977-3 [60/0/-60]3S unnotched compression, Sun | quasi-isotropic | 765 | 603.11 | −21.2 % |
| IM7/977-3 [60/0/-60]3S unnotched compression, Edge | quasi-isotropic | 765 | 603.11 | −21.2 % |
| IM7/977-3 [60/0/-60]3S unnotched compression, Max Strain | quasi-isotropic | 765 | 603.26 | −21.1 % |
| IM7/977-3 [60/0/-60]3S unnotched compression, Tsai-Hill | quasi-isotropic | 765 | 603.34 | −21.1 % |
| IM7/977-3 [60/0/-60]3S unnotched compression, Tsai-Wu | quasi-isotropic | 765 | 609.69 | −20.3 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression, Edge | angle-ply | 382 | 307.99 | −19.4 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension, Tsai-Hill | angle-ply | 473 | 381.47 | −19.4 % |
| IM7/977-3 [0/45/90/-45]2S unnotched tension, Tsai-Hill | quasi-isotropic | 866 | 726.25 | −16.1 % |
| IM7/977-3 [0/45/90/-45]2S unnotched tension, Tsai-Wu | quasi-isotropic | 866 | 726.25 | −16.1 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched compression, Tsai-Hill | angle-ply | 382 | 435.77 | +14.1 % |
| IM7/977-3 [0/45/90/-45]2S unnotched tension, Max Stress | quasi-isotropic | 866 | 968.56 | +11.8 % |
| IM7/977-3 [0/45/90/-45]2S unnotched tension, Hashin | quasi-isotropic | 866 | 968.56 | +11.8 % |
| IM7/977-3 [0/45/90/-45]2S unnotched tension, Puck | quasi-isotropic | 866 | 968.56 | +11.8 % |
| IM7/977-3 [0/45/90/-45]2S unnotched tension, Sun | quasi-isotropic | 866 | 968.56 | +11.8 % |
| IM7/977-3 [0/45/90/-45]2S unnotched tension, Edge | quasi-isotropic | 866 | 968.56 | +11.8 % |
| IM7/977-3 [0/45/90/-45]2S unnotched tension, Cuntze (FMC) | quasi-isotropic | 866 | 968.56 | +11.8 % |
| IM7/977-3 [0/45/90/-45]2S unnotched tension, Max Strain | quasi-isotropic | 866 | 968.34 | +11.8 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression, Edge | quasi-isotropic | 603 | 543.3 | −9.90 % |
| IM7/977-3 [30/60/90/-60/-30]2S unnotched tension, Hashin | angle-ply | 473 | 516.66 | +9.23 % |
| IM7/977-3 [60/0/-60]3S unnotched tension, Tsai-Hill | quasi-isotropic | 1005 | 968.33 | −3.65 % |
| IM7/977-3 [60/0/-60]3S unnotched tension, Tsai-Wu | quasi-isotropic | 1005 | 968.33 | −3.65 % |
| IM7/977-3 [60/0/-60]3S unnotched tension, Max Strain | quasi-isotropic | 1005 | 968.34 | −3.65 % |
| IM7/977-3 [60/0/-60]3S unnotched tension, Cuntze (FMC) | quasi-isotropic | 1005 | 968.56 | −3.63 % |
| IM7/977-3 [60/0/-60]3S unnotched tension, Max Stress | quasi-isotropic | 1005 | 968.56 | −3.63 % |
| IM7/977-3 [60/0/-60]3S unnotched tension, Hashin | quasi-isotropic | 1005 | 968.56 | −3.63 % |
| IM7/977-3 [60/0/-60]3S unnotched tension, Puck | quasi-isotropic | 1005 | 968.56 | −3.63 % |
| IM7/977-3 [60/0/-60]3S unnotched tension, Sun | quasi-isotropic | 1005 | 968.56 | −3.63 % |
| IM7/977-3 [60/0/-60]3S unnotched tension, Edge | quasi-isotropic | 1005 | 968.56 | −3.63 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression, Tsai-Wu | quasi-isotropic | 603 | 609.69 | +1.11 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression, Tsai-Hill | quasi-isotropic | 603 | 603.34 | +0.056 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression, Max Strain | quasi-isotropic | 603 | 603.26 | +0.043 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression, Max Stress | quasi-isotropic | 603 | 603.11 | +0.019 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression, Hashin | quasi-isotropic | 603 | 603.11 | +0.019 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression, Puck | quasi-isotropic | 603 | 603.11 | +0.019 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression, Sun | quasi-isotropic | 603 | 603.11 | +0.019 % |
| IM7/977-3 [0/45/90/-45]2S unnotched compression, Cuntze (FMC) | quasi-isotropic | 603 | 603.11 | +0.019 % |
Soden, P. D., Hinton, M. J. & Kaddour, A. S., Biaxial Test Results for Strength and Deformation of a Range of E-Glass and Carbon Fibre Reinforced Composite Laminates: Failure Exercise Benchmark Data, Compos. Sci. Technol. 62 (2002) 1489-1514. Lamina properties from Soden, Hinton & Kaddour, Compos. Sci. Technol. 58 (1998) 1011-1022, Table 1.
Measured [MPa]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 55.2 | 80 | +44.9 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 767.97 | 472.74 | −38.4 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 181.64 | 251.41 | +38.4 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 990.98 | 616.15 | −37.8 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 660.46 | 900.76 | +36.4 % | Known gap |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 908.47 | 1222.2 | +34.5 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 823.39 | 568.86 | −30.9 % | Known gap |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 838.84 | 1086.1 | +29.5 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 724.25 | 532.16 | −26.5 % | Known gap |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 704.48 | 887.67 | +26.0 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 63.5 | 80 | +26.0 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 64.6 | 80 | +23.8 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 315.6 | 241.61 | −23.4 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 735.6 | 900 | +22.3 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 101.3 | 80 | −21.0 % | Known gap |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 66.5 | 80 | +20.3 % | Known gap |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19 failure stress magnitude [MPa], Puck | 524.16 | 628.12 | +19.8 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7 failure stress magnitude [MPa], Puck | 142 | 114 | −19.7 % | Over 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 680.11 | 805.08 | +18.4 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16 failure stress magnitude [MPa], Puck | 61.2 | 72 | +17.6 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6 failure stress magnitude [MPa], Puck | 137.8 | 114 | −17.3 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10 failure stress magnitude [MPa], Puck | 137.67 | 114.19 | −17.1 % | Over 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 157.62 | 133.15 | −15.5 % | Over 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 478.84 | 404.94 | −15.4 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15 failure stress magnitude [MPa], Puck | 134.9 | 114.1 | −15.4 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 133.66 | 114.39 | −14.4 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8 failure stress magnitude [MPa], Puck | 132.3 | 114 | −13.8 % | Over 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1 failure stress magnitude [MPa], Puck | 1318.9 | 1500 | +13.7 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 119.59 | 103.93 | −13.1 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1 failure stress magnitude [MPa], Puck | 40 | 35 | −12.5 % | Over 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14 failure stress magnitude [MPa], Puck | 1139.5 | 1281.7 | +12.5 % | Over 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1437.3 | 1261.3 | −12.2 % | Over 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 799.58 | 893.96 | +11.8 % | Over 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1200.6 | 1063.8 | −11.4 % | Over 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1117.8 | 1233.6 | +10.4 % | Over 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 54.366 | 59.996 | +10.4 % | Over 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1181.5 | 1069.3 | −9.50 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5 failure stress magnitude [MPa], Puck | 1376.4 | 1500.4 | +9.00 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1418.9 | 1293.9 | −8.82 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 791.48 | 854.82 | +8.00 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1170.5 | 1078 | −7.90 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34 failure stress magnitude [MPa], Puck | 835.7 | 900 | +7.69 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1029.4 | 1104.7 | +7.31 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25 failure stress magnitude [MPa], Puck | 86.3 | 80 | −7.30 % | Within 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 44.94 | 48.139 | +7.12 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13 failure stress magnitude [MPa], Puck | 1200.7 | 1280.8 | +6.67 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 274.04 | 255.82 | −6.65 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20 failure stress magnitude [MPa], Puck | 246.84 | 263.18 | +6.62 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 1041.4 | 1109.7 | +6.56 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23 failure stress magnitude [MPa], Puck | 854.8 | 900 | +5.29 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6 failure stress magnitude [MPa], Puck | 1134.5 | 1077 | −5.07 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24 failure stress magnitude [MPa], Puck | 939.3 | 900 | −4.18 % | Within 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 118.49 | 113.91 | −3.87 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11 failure stress magnitude [MPa], Puck | 1124.5 | 1086.6 | −3.37 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 420.61 | 406.88 | −3.26 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7 failure stress magnitude [MPa], Puck | 1311 | 1347.9 | +2.81 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12 failure stress magnitude [MPa], Puck | 1249 | 1280 | +2.48 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6 failure stress magnitude [MPa], Puck | 1481.3 | 1458 | −1.57 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4 failure stress magnitude [MPa], Puck | 1522.9 | 1500.1 | −1.50 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2 failure stress magnitude [MPa], Puck | 1481.1 | 1500 | +1.28 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7 failure stress magnitude [MPa], Puck | 1086.4 | 1099.1 | +1.17 % | Within 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4 failure stress magnitude [MPa], Puck | 36.33 | 36.706 | +1.04 % | Within 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 93.018 | 93.52 | +0.54 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 565.09 | 562.76 | −0.41 % | Within 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3 failure stress magnitude [MPa], Puck | 44.562 | 44.642 | +0.18 % | Within 10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9 failure stress magnitude [MPa], Puck | 114.55 | 114.39 | −0.14 % | Within 10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3 failure stress magnitude [MPa], Puck | 1500.7 | 1500 | −0.047 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1 failure stress magnitude [MPa], Puck | 40 | 40 | <0.001 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2 failure stress magnitude [MPa], Puck | 1280 | 1280 | <0.001 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3 failure stress magnitude [MPa], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 800 | 800 | <0.001 % | Within 10 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21 failure stress magnitude [MPa], Puck | 145 | 145 | <0.001 % | Within 10 % |
How to reproduce it
Source
Soden, P. D., Hinton, M. J. & Kaddour, A. S., Biaxial Test Results for Strength and Deformation of a Range of E-Glass and Carbon Fibre Reinforced Composite Laminates: Failure Exercise Benchmark Data, Compos. Sci. Technol. 62 (2002) 1489-1514. Lamina properties from Soden, Hinton & Kaddour, Compos. Sci. Technol. 58 (1998) 1011-1022, Table 1.
Tables 1, 2 and 3
What was taken from it
The measured biaxial failure stresses of the E-glass/LY556 (σ<sub>2</sub> and τ<sub>12</sub>), T300/BSL914C (σ<sub>1</sub> and τ<sub>12</sub>) and E-glass/MY750 (σ<sub>1</sub> and σ<sub>2</sub>) tubes.
Quantity compared: failure stress magnitude [MPa]
Inputs
- Each tube is a single ply under the measured stress state. The load grows along the measured stress ratio until the first-ply failure criterion reaches 1.
- Compared value: the failure stress magnitude along that ratio, MPa.
- Every failure criterion the app has is a sub-case of each test, run with the app's default parameters. Nothing is tuned to the test and no cure residual stress is applied.
- The lamina strengths are the exercise's benchmark inputs. Soden et al. (1998) call them typical values derived by a variety of methods, so they are not the strengths of the tubes that were tested.
The inputs of each configuration are listed in the table below.
Allowed difference
±20 %; outside it, known gap
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10, Edge | unidirectional | 990.98 | 378.03 | −61.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13, Edge | unidirectional | 767.97 | 311.58 | −59.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11, Edge | unidirectional | 823.39 | 355.11 | −56.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17, Max Stress | unidirectional | 838.84 | 1287.4 | +53.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17, Hashin | unidirectional | 838.84 | 1287.4 | +53.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17, Sun | unidirectional | 838.84 | 1287.4 | +53.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17, Edge | unidirectional | 838.84 | 1287.4 | +53.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12, Edge | unidirectional | 724.25 | 338.12 | −53.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10, Tsai-Wu | unidirectional | 990.98 | 500.61 | −49.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3, Max Strain | unidirectional | 800 | 405.01 | −49.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13, Tsai-Wu | unidirectional | 767.97 | 398.77 | −48.1 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10, Tsai-Hill | unidirectional | 990.98 | 527.37 | −46.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13, Tsai-Hill | unidirectional | 767.97 | 419.97 | −45.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15, Cuntze (FMC) | unidirectional | 55.2 | 80 | +44.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15, Max Stress | unidirectional | 55.2 | 80 | +44.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15, Max Strain | unidirectional | 55.2 | 80 | +44.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15, Tsai-Hill | unidirectional | 55.2 | 80 | +44.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15, Tsai-Wu | unidirectional | 55.2 | 80 | +44.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15, Hashin | unidirectional | 55.2 | 80 | +44.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15, Puck | unidirectional | 55.2 | 80 | +44.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15, Sun | unidirectional | 55.2 | 80 | +44.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 15, Edge | unidirectional | 55.2 | 80 | +44.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11, Tsai-Wu | unidirectional | 823.39 | 465.47 | −43.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10, Cuntze (FMC) | unidirectional | 990.98 | 561.52 | −43.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13, Cuntze (FMC) | unidirectional | 767.97 | 440.72 | −42.6 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20, Edge | unidirectional | 478.84 | 281 | −41.3 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16, Max Stress | unidirectional | 908.47 | 1283.5 | +41.3 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16, Hashin | unidirectional | 908.47 | 1283.5 | +41.3 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16, Sun | unidirectional | 908.47 | 1283.5 | +41.3 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16, Edge | unidirectional | 908.47 | 1283.5 | +41.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11, Tsai-Hill | unidirectional | 823.39 | 490.64 | −40.4 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5, Max Stress | unidirectional | 54.366 | 76.304 | +40.4 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5, Max Strain | unidirectional | 54.366 | 76.304 | +40.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12, Tsai-Wu | unidirectional | 724.25 | 439.38 | −39.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19, Edge | unidirectional | 315.6 | 192.78 | −38.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13, Puck | unidirectional | 767.97 | 472.74 | −38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13, Max Stress | unidirectional | 767.97 | 472.96 | −38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13, Max Strain | unidirectional | 767.97 | 472.96 | −38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13, Hashin | unidirectional | 767.97 | 472.96 | −38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 13, Sun | unidirectional | 767.97 | 472.96 | −38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14, Max Stress | unidirectional | 181.64 | 251.41 | +38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14, Max Strain | unidirectional | 181.64 | 251.41 | +38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14, Hashin | unidirectional | 181.64 | 251.41 | +38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14, Puck | unidirectional | 181.64 | 251.41 | +38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14, Sun | unidirectional | 181.64 | 251.41 | +38.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10, Puck | unidirectional | 990.98 | 616.15 | −37.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30, Edge | unidirectional | 565.09 | 352.24 | −37.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11, Cuntze (FMC) | unidirectional | 823.39 | 520.14 | −36.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14, Cuntze (FMC) | unidirectional | 181.64 | 247.87 | +36.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32, Max Stress | unidirectional | 660.46 | 900.76 | +36.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32, Max Strain | unidirectional | 660.46 | 900.76 | +36.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32, Hashin | unidirectional | 660.46 | 900.76 | +36.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32, Puck | unidirectional | 660.46 | 900.76 | +36.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32, Sun | unidirectional | 660.46 | 900.76 | +36.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12, Tsai-Hill | unidirectional | 724.25 | 463.12 | −36.1 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10, Max Stress | unidirectional | 990.98 | 648.23 | −34.6 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10, Max Strain | unidirectional | 990.98 | 648.23 | −34.6 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10, Hashin | unidirectional | 990.98 | 648.23 | −34.6 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 10, Sun | unidirectional | 990.98 | 648.23 | −34.6 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16, Puck | unidirectional | 908.47 | 1222.2 | +34.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14, Tsai-Hill | unidirectional | 181.64 | 243.03 | +33.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18, Max Stress | unidirectional | 704.48 | 937.16 | +33.0 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18, Hashin | unidirectional | 704.48 | 937.16 | +33.0 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18, Sun | unidirectional | 704.48 | 937.16 | +33.0 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18, Edge | unidirectional | 704.48 | 937.16 | +33.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29, Edge | unidirectional | 420.61 | 281.92 | −33.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31, Max Stress | unidirectional | 680.11 | 902.4 | +32.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31, Max Strain | unidirectional | 680.11 | 902.4 | +32.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31, Hashin | unidirectional | 680.11 | 902.4 | +32.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31, Sun | unidirectional | 680.11 | 902.4 | +32.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12, Cuntze (FMC) | unidirectional | 724.25 | 489.14 | −32.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12, Tsai-Hill | unidirectional | 119.59 | 80.95 | −32.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12, Hashin | unidirectional | 119.59 | 80.95 | −32.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21, Edge | unidirectional | 791.48 | 541.5 | −31.6 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11, Puck | unidirectional | 823.39 | 568.86 | −30.9 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2, Max Stress | unidirectional | 44.94 | 58.472 | +30.1 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2, Max Strain | unidirectional | 44.94 | 58.472 | +30.1 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17, Puck | unidirectional | 838.84 | 1086.1 | +29.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11, Max Stress | unidirectional | 823.39 | 582.93 | −29.2 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11, Max Strain | unidirectional | 823.39 | 582.93 | −29.2 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11, Hashin | unidirectional | 823.39 | 582.93 | −29.2 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 11, Sun | unidirectional | 823.39 | 582.93 | −29.2 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32, Cuntze (FMC) | unidirectional | 660.46 | 852.85 | +29.1 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14, Tsai-Wu | unidirectional | 181.64 | 233.83 | +28.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19, Tsai-Wu | unidirectional | 315.6 | 225.59 | −28.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31, Edge | unidirectional | 680.11 | 495.11 | −27.2 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12, Puck | unidirectional | 724.25 | 532.16 | −26.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28, Edge | unidirectional | 274.04 | 201.43 | −26.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20, Tsai-Wu | unidirectional | 478.84 | 352.54 | −26.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22, Edge | unidirectional | 799.58 | 590.12 | −26.2 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18, Puck | unidirectional | 704.48 | 887.67 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16, Max Stress | unidirectional | 63.5 | 80 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16, Max Strain | unidirectional | 63.5 | 80 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16, Tsai-Hill | unidirectional | 63.5 | 80 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16, Tsai-Wu | unidirectional | 63.5 | 80 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16, Hashin | unidirectional | 63.5 | 80 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16, Puck | unidirectional | 63.5 | 80 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16, Cuntze (FMC) | unidirectional | 63.5 | 80 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16, Sun | unidirectional | 63.5 | 80 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 16, Edge | unidirectional | 63.5 | 80 | +26.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19, Tsai-Hill | unidirectional | 315.6 | 234.21 | −25.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12, Max Stress | unidirectional | 724.25 | 537.98 | −25.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12, Max Strain | unidirectional | 724.25 | 537.98 | −25.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12, Hashin | unidirectional | 724.25 | 537.98 | −25.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 12, Sun | unidirectional | 724.25 | 537.98 | −25.7 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16, Cuntze (FMC) | unidirectional | 908.47 | 1140.2 | +25.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12, Max Stress | unidirectional | 119.59 | 89.136 | −25.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12, Max Strain | unidirectional | 119.59 | 89.136 | −25.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12, Edge | unidirectional | 119.59 | 89.136 | −25.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9, Max Strain | unidirectional | 1029.4 | 1290.6 | +25.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9, Tsai-Hill | unidirectional | 1437.3 | 1082 | −24.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9, Hashin | unidirectional | 1437.3 | 1082 | −24.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27, Edge | unidirectional | 157.62 | 119.07 | −24.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19, Cuntze (FMC) | unidirectional | 315.6 | 238.56 | −24.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9, Max Stress | unidirectional | 1029.4 | 1280.5 | +24.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9, Hashin | unidirectional | 1029.4 | 1280.5 | +24.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9, Sun | unidirectional | 1029.4 | 1280.5 | +24.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9, Edge | unidirectional | 1029.4 | 1280.5 | +24.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5, Max Strain | unidirectional | 1041.4 | 1290.5 | +23.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17, Max Stress | unidirectional | 64.6 | 80 | +23.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17, Max Strain | unidirectional | 64.6 | 80 | +23.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17, Tsai-Hill | unidirectional | 64.6 | 80 | +23.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17, Tsai-Wu | unidirectional | 64.6 | 80 | +23.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17, Hashin | unidirectional | 64.6 | 80 | +23.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17, Puck | unidirectional | 64.6 | 80 | +23.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17, Cuntze (FMC) | unidirectional | 64.6 | 80 | +23.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17, Sun | unidirectional | 64.6 | 80 | +23.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 17, Edge | unidirectional | 64.6 | 80 | +23.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13, Tsai-Hill | unidirectional | 133.66 | 101.91 | −23.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13, Hashin | unidirectional | 133.66 | 101.91 | −23.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32, Tsai-Hill | unidirectional | 660.46 | 817.18 | +23.7 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10, Tsai-Hill | unidirectional | 1200.6 | 918.79 | −23.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19, Max Stress | unidirectional | 315.6 | 241.61 | −23.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19, Max Strain | unidirectional | 315.6 | 241.61 | −23.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19, Hashin | unidirectional | 315.6 | 241.61 | −23.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19, Puck | unidirectional | 315.6 | 241.61 | −23.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 19, Sun | unidirectional | 315.6 | 241.61 | −23.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15, Max Strain | unidirectional | 1117.8 | 857.02 | −23.3 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5, Max Stress | unidirectional | 1041.4 | 1280.5 | +23.0 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5, Hashin | unidirectional | 1041.4 | 1280.5 | +23.0 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5, Sun | unidirectional | 1041.4 | 1280.5 | +23.0 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5, Edge | unidirectional | 1041.4 | 1280.5 | +23.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20, Tsai-Hill | unidirectional | 478.84 | 370.5 | −22.6 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33, Max Stress | unidirectional | 735.6 | 900 | +22.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33, Max Strain | unidirectional | 735.6 | 900 | +22.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33, Tsai-Hill | unidirectional | 735.6 | 900 | +22.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33, Tsai-Wu | unidirectional | 735.6 | 900 | +22.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33, Hashin | unidirectional | 735.6 | 900 | +22.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33, Puck | unidirectional | 735.6 | 900 | +22.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33, Cuntze (FMC) | unidirectional | 735.6 | 900 | +22.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33, Sun | unidirectional | 735.6 | 900 | +22.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 33, Edge | unidirectional | 735.6 | 900 | +22.3 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8, Tsai-Hill | unidirectional | 1181.5 | 923.95 | −21.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14, Cuntze (FMC) | unidirectional | 93.018 | 113.11 | +21.6 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8, Tsai-Hill | unidirectional | 1418.9 | 1113.5 | −21.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8, Hashin | unidirectional | 1418.9 | 1113.5 | −21.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32, Tsai-Wu | unidirectional | 660.46 | 800.91 | +21.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5, Cuntze (FMC) | unidirectional | 54.366 | 65.899 | +21.2 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26, Cuntze (FMC) | unidirectional | 101.3 | 80 | −21.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26, Max Stress | unidirectional | 101.3 | 80 | −21.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26, Max Strain | unidirectional | 101.3 | 80 | −21.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26, Tsai-Hill | unidirectional | 101.3 | 80 | −21.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26, Tsai-Wu | unidirectional | 101.3 | 80 | −21.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26, Hashin | unidirectional | 101.3 | 80 | −21.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26, Puck | unidirectional | 101.3 | 80 | −21.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26, Sun | unidirectional | 101.3 | 80 | −21.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 26, Edge | unidirectional | 101.3 | 80 | −21.0 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4, Tsai-Hill | unidirectional | 1170.5 | 932.36 | −20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9, Tsai-Wu | unidirectional | 1437.3 | 1145.5 | −20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18, Max Stress | unidirectional | 66.5 | 80 | +20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18, Max Strain | unidirectional | 66.5 | 80 | +20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18, Tsai-Hill | unidirectional | 66.5 | 80 | +20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18, Tsai-Wu | unidirectional | 66.5 | 80 | +20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18, Hashin | unidirectional | 66.5 | 80 | +20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18, Puck | unidirectional | 66.5 | 80 | +20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18, Cuntze (FMC) | unidirectional | 66.5 | 80 | +20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18, Sun | unidirectional | 66.5 | 80 | +20.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 18, Edge | unidirectional | 66.5 | 80 | +20.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11, Tsai-Hill | unidirectional | 118.49 | 94.786 | −20.0 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11, Hashin | unidirectional | 118.49 | 94.786 | −20.0 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19, Max Stress | unidirectional | 524.16 | 628.12 | +19.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19, Hashin | unidirectional | 524.16 | 628.12 | +19.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19, Puck | unidirectional | 524.16 | 628.12 | +19.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19, Sun | unidirectional | 524.16 | 628.12 | +19.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19, Edge | unidirectional | 524.16 | 628.12 | +19.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10, Tsai-Hill | unidirectional | 137.67 | 110.39 | −19.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10, Hashin | unidirectional | 137.67 | 110.39 | −19.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7, Cuntze (FMC) | unidirectional | 142 | 114 | −19.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7, Max Stress | unidirectional | 142 | 114 | −19.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7, Max Strain | unidirectional | 142 | 114 | −19.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7, Tsai-Hill | unidirectional | 142 | 114 | −19.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7, Tsai-Wu | unidirectional | 142 | 114 | −19.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7, Hashin | unidirectional | 142 | 114 | −19.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7, Puck | unidirectional | 142 | 114 | −19.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7, Sun | unidirectional | 142 | 114 | −19.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 7, Edge | unidirectional | 142 | 114 | −19.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20, Cuntze (FMC) | unidirectional | 478.84 | 385.73 | −19.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9, Cuntze (FMC) | unidirectional | 1437.3 | 1159.6 | −19.3 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17, Cuntze (FMC) | unidirectional | 838.84 | 998.93 | +19.1 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7, Max Strain | unidirectional | 1086.4 | 1290.8 | +18.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10, Cuntze (FMC) | unidirectional | 1200.6 | 977 | −18.6 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18, Max Strain | unidirectional | 704.48 | 574.72 | −18.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30, Tsai-Wu | unidirectional | 565.09 | 461.08 | −18.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31, Puck | unidirectional | 680.11 | 805.08 | +18.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6, Tsai-Hill | unidirectional | 1134.5 | 931.35 | −17.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7, Max Stress | unidirectional | 1086.4 | 1280.5 | +17.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7, Hashin | unidirectional | 1086.4 | 1280.5 | +17.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7, Sun | unidirectional | 1086.4 | 1280.5 | +17.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7, Edge | unidirectional | 1086.4 | 1280.5 | +17.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27, Tsai-Wu | unidirectional | 157.62 | 129.51 | −17.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16, Max Stress | unidirectional | 61.2 | 72 | +17.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16, Max Strain | unidirectional | 61.2 | 72 | +17.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16, Tsai-Hill | unidirectional | 61.2 | 72 | +17.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16, Tsai-Wu | unidirectional | 61.2 | 72 | +17.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16, Hashin | unidirectional | 61.2 | 72 | +17.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16, Puck | unidirectional | 61.2 | 72 | +17.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16, Sun | unidirectional | 61.2 | 72 | +17.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16, Edge | unidirectional | 61.2 | 72 | +17.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 16, Cuntze (FMC) | unidirectional | 61.2 | 72 | +17.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10, Tsai-Wu | unidirectional | 137.67 | 113.54 | −17.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6, Sun | unidirectional | 137.8 | 114 | −17.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6, Max Stress | unidirectional | 137.8 | 114 | −17.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6, Max Strain | unidirectional | 137.8 | 114 | −17.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6, Tsai-Hill | unidirectional | 137.8 | 114 | −17.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6, Tsai-Wu | unidirectional | 137.8 | 114 | −17.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6, Hashin | unidirectional | 137.8 | 114 | −17.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6, Puck | unidirectional | 137.8 | 114 | −17.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6, Cuntze (FMC) | unidirectional | 137.8 | 114 | −17.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 6, Edge | unidirectional | 137.8 | 114 | −17.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8, Tsai-Wu | unidirectional | 1418.9 | 1175 | −17.2 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10, Puck | unidirectional | 137.67 | 114.19 | −17.1 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15, Tsai-Hill | unidirectional | 134.9 | 112.03 | −17.0 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15, Hashin | unidirectional | 134.9 | 112.03 | −17.0 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10, Sun | unidirectional | 137.67 | 114.45 | −16.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8, Cuntze (FMC) | unidirectional | 1181.5 | 982.46 | −16.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14, Tsai-Hill | unidirectional | 93.018 | 77.42 | −16.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14, Hashin | unidirectional | 93.018 | 77.42 | −16.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11, Tsai-Hill | unidirectional | 1124.5 | 940.64 | −16.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13, Tsai-Wu | unidirectional | 133.66 | 112.03 | −16.2 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27, Tsai-Hill | unidirectional | 157.62 | 132.23 | −16.1 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8, Cuntze (FMC) | unidirectional | 1418.9 | 1192.7 | −15.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17, Max Strain | unidirectional | 838.84 | 705.65 | −15.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29, Tsai-Wu | unidirectional | 420.61 | 353.91 | −15.9 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2, Cuntze (FMC) | unidirectional | 44.94 | 51.991 | +15.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27, Cuntze (FMC) | unidirectional | 157.62 | 132.9 | −15.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15, Tsai-Wu | unidirectional | 134.9 | 113.76 | −15.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27, Max Stress | unidirectional | 157.62 | 133.15 | −15.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27, Max Strain | unidirectional | 157.62 | 133.15 | −15.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27, Hashin | unidirectional | 157.62 | 133.15 | −15.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27, Puck | unidirectional | 157.62 | 133.15 | −15.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 27, Sun | unidirectional | 157.62 | 133.15 | −15.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20, Max Stress | unidirectional | 478.84 | 404.94 | −15.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20, Max Strain | unidirectional | 478.84 | 404.94 | −15.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20, Hashin | unidirectional | 478.84 | 404.94 | −15.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20, Puck | unidirectional | 478.84 | 404.94 | −15.4 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 20, Sun | unidirectional | 478.84 | 404.94 | −15.4 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15, Puck | unidirectional | 134.9 | 114.1 | −15.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14, Max Strain | unidirectional | 1139.5 | 964.05 | −15.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19, Max Strain | unidirectional | 524.16 | 443.5 | −15.4 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12, Tsai-Wu | unidirectional | 119.59 | 101.21 | −15.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16, Tsai-Hill | unidirectional | 908.47 | 1047.9 | +15.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4, Cuntze (FMC) | unidirectional | 1170.5 | 991.33 | −15.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15, Sun | unidirectional | 134.9 | 114.25 | −15.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10, Cuntze (FMC) | unidirectional | 137.67 | 116.6 | −15.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10, Max Stress | unidirectional | 137.67 | 116.6 | −15.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10, Max Strain | unidirectional | 137.67 | 116.6 | −15.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 10, Edge | unidirectional | 137.67 | 116.6 | −15.3 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11, Max Strain | unidirectional | 1124.5 | 1291.1 | +14.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18, Cuntze (FMC) | unidirectional | 704.48 | 808.85 | +14.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15, Max Stress | unidirectional | 1117.8 | 1283.2 | +14.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15, Hashin | unidirectional | 1117.8 | 1283.2 | +14.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15, Sun | unidirectional | 1117.8 | 1283.2 | +14.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15, Edge | unidirectional | 1117.8 | 1283.2 | +14.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11, Cuntze (FMC) | unidirectional | 118.49 | 135.81 | +14.6 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7, Max Stress | unidirectional | 1311 | 1501.4 | +14.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7, Max Strain | unidirectional | 1311 | 1501.4 | +14.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7, Sun | unidirectional | 1311 | 1501.4 | +14.5 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7, Edge | unidirectional | 1311 | 1501.4 | +14.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15, Max Stress | unidirectional | 134.9 | 115.37 | −14.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15, Max Strain | unidirectional | 134.9 | 115.37 | −14.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15, Cuntze (FMC) | unidirectional | 134.9 | 115.37 | −14.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 15, Edge | unidirectional | 134.9 | 115.37 | −14.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13, Puck | unidirectional | 133.66 | 114.39 | −14.4 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3, Max Stress | unidirectional | 44.562 | 50.804 | +14.0 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3, Max Strain | unidirectional | 44.562 | 50.804 | +14.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30, Tsai-Hill | unidirectional | 565.09 | 486.01 | −14.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21, Max Stress | unidirectional | 791.48 | 901.57 | +13.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21, Max Strain | unidirectional | 791.48 | 901.57 | +13.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21, Hashin | unidirectional | 791.48 | 901.57 | +13.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21, Sun | unidirectional | 791.48 | 901.57 | +13.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11, Max Stress | unidirectional | 1124.5 | 1280.6 | +13.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11, Hashin | unidirectional | 1124.5 | 1280.6 | +13.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11, Sun | unidirectional | 1124.5 | 1280.6 | +13.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11, Edge | unidirectional | 1124.5 | 1280.6 | +13.9 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8, Sun | unidirectional | 132.3 | 114 | −13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8, Max Stress | unidirectional | 132.3 | 114 | −13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8, Max Strain | unidirectional | 132.3 | 114 | −13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8, Tsai-Hill | unidirectional | 132.3 | 114 | −13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8, Tsai-Wu | unidirectional | 132.3 | 114 | −13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8, Hashin | unidirectional | 132.3 | 114 | −13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8, Puck | unidirectional | 132.3 | 114 | −13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8, Cuntze (FMC) | unidirectional | 132.3 | 114 | −13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 8, Edge | unidirectional | 132.3 | 114 | −13.8 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6, Max Strain | unidirectional | 1134.5 | 1291.3 | +13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5, Tsai-Hill | unidirectional | 54.366 | 61.87 | +13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5, Hashin | unidirectional | 54.366 | 61.87 | +13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5, Sun | unidirectional | 54.366 | 61.87 | +13.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5, Edge | unidirectional | 54.366 | 61.87 | +13.8 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1, Max Stress | unidirectional | 1318.9 | 1500 | +13.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1, Max Strain | unidirectional | 1318.9 | 1500 | +13.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1, Tsai-Hill | unidirectional | 1318.9 | 1500 | +13.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1, Tsai-Wu | unidirectional | 1318.9 | 1500 | +13.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1, Hashin | unidirectional | 1318.9 | 1500 | +13.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1, Puck | unidirectional | 1318.9 | 1500 | +13.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1, Cuntze (FMC) | unidirectional | 1318.9 | 1500 | +13.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1, Sun | unidirectional | 1318.9 | 1500 | +13.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 1, Edge | unidirectional | 1318.9 | 1500 | +13.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13, Sun | unidirectional | 133.66 | 115.31 | −13.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28, Tsai-Wu | unidirectional | 274.04 | 237.52 | −13.3 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12, Puck | unidirectional | 119.59 | 103.93 | −13.1 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19, Cuntze (FMC) | unidirectional | 524.16 | 592.42 | +13.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6, Tsai-Hill | unidirectional | 1481.3 | 1290.3 | −12.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6, Hashin | unidirectional | 1481.3 | 1290.3 | −12.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6, Max Stress | unidirectional | 1134.5 | 1280.6 | +12.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6, Hashin | unidirectional | 1134.5 | 1280.6 | +12.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6, Sun | unidirectional | 1134.5 | 1280.6 | +12.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6, Edge | unidirectional | 1134.5 | 1280.6 | +12.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6, Cuntze (FMC) | unidirectional | 1134.5 | 990.27 | −12.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22, Max Stress | unidirectional | 799.58 | 900.99 | +12.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22, Max Strain | unidirectional | 799.58 | 900.99 | +12.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22, Hashin | unidirectional | 799.58 | 900.99 | +12.7 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22, Sun | unidirectional | 799.58 | 900.99 | +12.7 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1, Max Stress | unidirectional | 40 | 35 | −12.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1, Max Strain | unidirectional | 40 | 35 | −12.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1, Tsai-Hill | unidirectional | 40 | 35 | −12.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1, Tsai-Wu | unidirectional | 40 | 35 | −12.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1, Hashin | unidirectional | 40 | 35 | −12.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1, Puck | unidirectional | 40 | 35 | −12.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1, Cuntze (FMC) | unidirectional | 40 | 35 | −12.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1, Sun | unidirectional | 40 | 35 | −12.5 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 1, Edge | unidirectional | 40 | 35 | −12.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14, Max Stress | unidirectional | 1139.5 | 1281.7 | +12.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14, Hashin | unidirectional | 1139.5 | 1281.7 | +12.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14, Puck | unidirectional | 1139.5 | 1281.7 | +12.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14, Sun | unidirectional | 1139.5 | 1281.7 | +12.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14, Edge | unidirectional | 1139.5 | 1281.7 | +12.5 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7, Tsai-Hill | unidirectional | 1086.4 | 952.9 | −12.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9, Puck | unidirectional | 1437.3 | 1261.3 | −12.2 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14, Max Stress | unidirectional | 93.018 | 81.774 | −12.1 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14, Max Strain | unidirectional | 93.018 | 81.774 | −12.1 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14, Edge | unidirectional | 93.018 | 81.774 | −12.1 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22, Puck | unidirectional | 799.58 | 893.96 | +11.8 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11, Max Stress | unidirectional | 118.49 | 132.27 | +11.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11, Max Strain | unidirectional | 118.49 | 132.27 | +11.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11, Edge | unidirectional | 118.49 | 132.27 | +11.6 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12, Sun | unidirectional | 119.59 | 105.69 | −11.6 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29, Tsai-Hill | unidirectional | 420.61 | 371.97 | −11.6 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10, Puck | unidirectional | 1200.6 | 1063.8 | −11.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11, Cuntze (FMC) | unidirectional | 1124.5 | 1000 | −11.1 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9, Tsai-Hill | unidirectional | 114.55 | 101.95 | −11.0 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9, Hashin | unidirectional | 114.55 | 101.95 | −11.0 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7, Tsai-Hill | unidirectional | 1311 | 1168.2 | −10.9 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7, Hashin | unidirectional | 1311 | 1168.2 | −10.9 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15, Tsai-Wu | unidirectional | 1117.8 | 999.84 | −10.6 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15, Puck | unidirectional | 1117.8 | 1233.6 | +10.4 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5, Puck | unidirectional | 54.366 | 59.996 | +10.4 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4, Max Strain | unidirectional | 1170.5 | 1291.3 | +10.3 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6, Tsai-Wu | unidirectional | 1481.3 | 1332.5 | −10.1 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28, Tsai-Hill | unidirectional | 274.04 | 246.97 | −9.88 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9, Tsai-Wu | unidirectional | 1029.4 | 1129.5 | +9.72 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13, Max Strain | unidirectional | 1200.7 | 1084.7 | −9.67 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 12, Cuntze (FMC) | unidirectional | 119.59 | 131.1 | +9.63 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31, Cuntze (FMC) | unidirectional | 680.11 | 745.18 | +9.57 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8, Puck | unidirectional | 1181.5 | 1069.3 | −9.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 14, Edge | unidirectional | 181.64 | 198.77 | +9.43 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4, Max Stress | unidirectional | 1170.5 | 1280.6 | +9.40 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4, Hashin | unidirectional | 1170.5 | 1280.6 | +9.40 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4, Sun | unidirectional | 1170.5 | 1280.6 | +9.40 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4, Edge | unidirectional | 1170.5 | 1280.6 | +9.40 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8, Max Strain | unidirectional | 1181.5 | 1291.5 | +9.31 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2, Tsai-Hill | unidirectional | 44.94 | 49.013 | +9.06 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2, Hashin | unidirectional | 44.94 | 49.013 | +9.06 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2, Sun | unidirectional | 44.94 | 49.013 | +9.06 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2, Edge | unidirectional | 44.94 | 49.013 | +9.06 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5, Max Stress | unidirectional | 1376.4 | 1500.4 | +9.00 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5, Max Strain | unidirectional | 1376.4 | 1500.4 | +9.00 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5, Puck | unidirectional | 1376.4 | 1500.4 | +9.00 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5, Sun | unidirectional | 1376.4 | 1500.4 | +9.00 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5, Edge | unidirectional | 1376.4 | 1500.4 | +9.00 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9, Max Stress | unidirectional | 114.55 | 124.85 | +8.99 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9, Max Strain | unidirectional | 114.55 | 124.85 | +8.99 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9, Cuntze (FMC) | unidirectional | 114.55 | 124.85 | +8.99 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9, Edge | unidirectional | 114.55 | 124.85 | +8.99 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30, Cuntze (FMC) | unidirectional | 565.09 | 514.92 | −8.88 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8, Puck | unidirectional | 1418.9 | 1293.9 | −8.82 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5, Tsai-Wu | unidirectional | 1041.4 | 1132.5 | +8.75 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8, Max Stress | unidirectional | 1181.5 | 1280.6 | +8.38 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8, Hashin | unidirectional | 1181.5 | 1280.6 | +8.38 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8, Sun | unidirectional | 1181.5 | 1280.6 | +8.38 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8, Edge | unidirectional | 1181.5 | 1280.6 | +8.38 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16, Tsai-Wu | unidirectional | 908.47 | 984.33 | +8.35 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21, Tsai-Wu | unidirectional | 791.48 | 726.92 | −8.16 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17, Tsai-Hill | unidirectional | 838.84 | 906.87 | +8.11 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10, Tsai-Wu | unidirectional | 1200.6 | 1103.9 | −8.05 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28, Cuntze (FMC) | unidirectional | 274.04 | 252.04 | −8.03 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21, Puck | unidirectional | 791.48 | 854.82 | +8.00 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6, Cuntze (FMC) | unidirectional | 1481.3 | 1363.1 | −7.98 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29, Cuntze (FMC) | unidirectional | 420.61 | 387.35 | −7.91 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4, Puck | unidirectional | 1170.5 | 1078 | −7.90 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34, Max Stress | unidirectional | 835.7 | 900 | +7.69 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34, Max Strain | unidirectional | 835.7 | 900 | +7.69 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34, Tsai-Hill | unidirectional | 835.7 | 900 | +7.69 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34, Tsai-Wu | unidirectional | 835.7 | 900 | +7.69 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34, Hashin | unidirectional | 835.7 | 900 | +7.69 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34, Puck | unidirectional | 835.7 | 900 | +7.69 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34, Cuntze (FMC) | unidirectional | 835.7 | 900 | +7.69 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34, Sun | unidirectional | 835.7 | 900 | +7.69 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 34, Edge | unidirectional | 835.7 | 900 | +7.69 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10, Max Strain | unidirectional | 1200.6 | 1291.7 | +7.59 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5, Tsai-Hill | unidirectional | 1041.4 | 963.34 | −7.50 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 16, Max Strain | unidirectional | 908.47 | 841.83 | −7.34 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9, Puck | unidirectional | 1029.4 | 1104.7 | +7.31 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25, Cuntze (FMC) | unidirectional | 86.3 | 80 | −7.30 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25, Max Stress | unidirectional | 86.3 | 80 | −7.30 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25, Max Strain | unidirectional | 86.3 | 80 | −7.30 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25, Tsai-Hill | unidirectional | 86.3 | 80 | −7.30 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25, Tsai-Wu | unidirectional | 86.3 | 80 | −7.30 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25, Hashin | unidirectional | 86.3 | 80 | −7.30 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25, Puck | unidirectional | 86.3 | 80 | −7.30 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25, Sun | unidirectional | 86.3 | 80 | −7.30 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 25, Edge | unidirectional | 86.3 | 80 | −7.30 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20, Max Strain | unidirectional | 246.84 | 228.93 | −7.26 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11, Tsai-Wu | unidirectional | 118.49 | 110.04 | −7.13 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2, Puck | unidirectional | 44.94 | 48.139 | +7.12 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9, Tsai-Hill | unidirectional | 1029.4 | 958.4 | −6.90 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 32, Edge | unidirectional | 660.46 | 615.4 | −6.82 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7, Cuntze (FMC) | unidirectional | 1086.4 | 1012.8 | −6.78 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14, Cuntze (FMC) | unidirectional | 1139.5 | 1215.5 | +6.67 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13, Max Stress | unidirectional | 1200.7 | 1280.8 | +6.67 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13, Hashin | unidirectional | 1200.7 | 1280.8 | +6.67 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13, Puck | unidirectional | 1200.7 | 1280.8 | +6.67 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13, Sun | unidirectional | 1200.7 | 1280.8 | +6.67 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13, Edge | unidirectional | 1200.7 | 1280.8 | +6.67 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10, Max Stress | unidirectional | 1200.6 | 1280.6 | +6.67 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10, Hashin | unidirectional | 1200.6 | 1280.6 | +6.67 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10, Sun | unidirectional | 1200.6 | 1280.6 | +6.67 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 10, Edge | unidirectional | 1200.6 | 1280.6 | +6.67 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28, Max Stress | unidirectional | 274.04 | 255.82 | −6.65 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28, Max Strain | unidirectional | 274.04 | 255.82 | −6.65 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28, Hashin | unidirectional | 274.04 | 255.82 | −6.65 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28, Puck | unidirectional | 274.04 | 255.82 | −6.65 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 28, Sun | unidirectional | 274.04 | 255.82 | −6.65 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20, Max Stress | unidirectional | 246.84 | 263.18 | +6.62 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20, Hashin | unidirectional | 246.84 | 263.18 | +6.62 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20, Puck | unidirectional | 246.84 | 263.18 | +6.62 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20, Sun | unidirectional | 246.84 | 263.18 | +6.62 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20, Edge | unidirectional | 246.84 | 263.18 | +6.62 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13, Max Stress | unidirectional | 133.66 | 124.9 | −6.56 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13, Max Strain | unidirectional | 133.66 | 124.9 | −6.56 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13, Cuntze (FMC) | unidirectional | 133.66 | 124.9 | −6.56 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 13, Edge | unidirectional | 133.66 | 124.9 | −6.56 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5, Puck | unidirectional | 1041.4 | 1109.7 | +6.56 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7, Tsai-Wu | unidirectional | 1311 | 1225.2 | −6.54 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3, Cuntze (FMC) | unidirectional | 44.562 | 47.436 | +6.45 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 8, Tsai-Wu | unidirectional | 1181.5 | 1107.3 | −6.28 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20, Cuntze (FMC) | unidirectional | 246.84 | 261.91 | +6.10 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8, Max Stress | unidirectional | 1418.9 | 1501.7 | +5.84 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8, Max Strain | unidirectional | 1418.9 | 1501.7 | +5.84 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8, Sun | unidirectional | 1418.9 | 1501.7 | +5.84 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 8, Edge | unidirectional | 1418.9 | 1501.7 | +5.84 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19, Tsai-Hill | unidirectional | 524.16 | 554.74 | +5.83 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23, Max Stress | unidirectional | 854.8 | 900 | +5.29 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23, Max Strain | unidirectional | 854.8 | 900 | +5.29 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23, Tsai-Hill | unidirectional | 854.8 | 900 | +5.29 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23, Tsai-Wu | unidirectional | 854.8 | 900 | +5.29 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23, Hashin | unidirectional | 854.8 | 900 | +5.29 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23, Puck | unidirectional | 854.8 | 900 | +5.29 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23, Sun | unidirectional | 854.8 | 900 | +5.29 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23, Edge | unidirectional | 854.8 | 900 | +5.29 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 23, Cuntze (FMC) | unidirectional | 854.8 | 900 | +5.29 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14, Sun | unidirectional | 93.018 | 97.83 | +5.17 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21, Tsai-Hill | unidirectional | 791.48 | 750.75 | −5.15 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6, Puck | unidirectional | 1134.5 | 1077 | −5.07 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15, Tsai-Hill | unidirectional | 1117.8 | 1061.2 | −5.06 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18, Tsai-Hill | unidirectional | 704.48 | 739.7 | +5.00 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 4, Tsai-Wu | unidirectional | 1170.5 | 1112.9 | −4.92 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7, Cuntze (FMC) | unidirectional | 1311 | 1248.5 | −4.77 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22, Cuntze (FMC) | unidirectional | 799.58 | 837.22 | +4.71 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 18, Tsai-Wu | unidirectional | 704.48 | 672.55 | −4.53 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9, Max Stress | unidirectional | 1437.3 | 1502 | +4.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9, Max Strain | unidirectional | 1437.3 | 1502 | +4.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9, Sun | unidirectional | 1437.3 | 1502 | +4.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 9, Edge | unidirectional | 1437.3 | 1502 | +4.50 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13, Cuntze (FMC) | unidirectional | 1200.7 | 1254.6 | +4.48 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4, Tsai-Hill | unidirectional | 1522.9 | 1454.9 | −4.46 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4, Hashin | unidirectional | 1522.9 | 1454.9 | −4.46 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5, Cuntze (FMC) | unidirectional | 1376.4 | 1436 | +4.32 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24, Cuntze (FMC) | unidirectional | 939.3 | 900 | −4.18 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24, Max Stress | unidirectional | 939.3 | 900 | −4.18 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24, Max Strain | unidirectional | 939.3 | 900 | −4.18 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24, Tsai-Hill | unidirectional | 939.3 | 900 | −4.18 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24, Tsai-Wu | unidirectional | 939.3 | 900 | −4.18 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24, Hashin | unidirectional | 939.3 | 900 | −4.18 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24, Puck | unidirectional | 939.3 | 900 | −4.18 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24, Sun | unidirectional | 939.3 | 900 | −4.18 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 24, Edge | unidirectional | 939.3 | 900 | −4.18 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20, Tsai-Hill | unidirectional | 246.84 | 256.97 | +4.10 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11, Puck | unidirectional | 118.49 | 113.91 | −3.87 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4, Tsai-Wu | unidirectional | 1522.9 | 1465.8 | −3.75 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7, Tsai-Wu | unidirectional | 1086.4 | 1126 | +3.64 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14, Tsai-Wu | unidirectional | 1139.5 | 1098.9 | −3.57 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 5, Tsai-Wu | unidirectional | 54.366 | 56.281 | +3.52 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11, Puck | unidirectional | 1124.5 | 1086.6 | −3.37 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14, Tsai-Wu | unidirectional | 93.018 | 96.126 | +3.34 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29, Max Stress | unidirectional | 420.61 | 406.88 | −3.26 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29, Max Strain | unidirectional | 420.61 | 406.88 | −3.26 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29, Hashin | unidirectional | 420.61 | 406.88 | −3.26 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29, Puck | unidirectional | 420.61 | 406.88 | −3.26 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 29, Sun | unidirectional | 420.61 | 406.88 | −3.26 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 19, Tsai-Wu | unidirectional | 524.16 | 507.17 | −3.24 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3, Tsai-Wu | unidirectional | 44.562 | 43.188 | −3.08 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 15, Cuntze (FMC) | unidirectional | 1117.8 | 1152.1 | +3.06 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4, Max Stress | unidirectional | 36.33 | 37.398 | +2.94 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4, Max Strain | unidirectional | 36.33 | 37.398 | +2.94 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 7, Puck | unidirectional | 1311 | 1347.9 | +2.81 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 11, Sun | unidirectional | 118.49 | 115.27 | −2.72 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4, Cuntze (FMC) | unidirectional | 1522.9 | 1481.6 | −2.72 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22, Tsai-Wu | unidirectional | 799.58 | 778.14 | −2.68 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12, Tsai-Wu | unidirectional | 1249 | 1281.6 | +2.61 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 2, Tsai-Wu | unidirectional | 44.94 | 46.092 | +2.56 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12, Max Stress | unidirectional | 1249 | 1280 | +2.48 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12, Hashin | unidirectional | 1249 | 1280 | +2.48 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12, Puck | unidirectional | 1249 | 1280 | +2.48 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12, Sun | unidirectional | 1249 | 1280 | +2.48 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12, Edge | unidirectional | 1249 | 1280 | +2.48 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12, Cuntze (FMC) | unidirectional | 1249 | 1279.9 | +2.48 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31, Tsai-Hill | unidirectional | 680.11 | 696.89 | +2.47 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12, Max Strain | unidirectional | 1249 | 1278.9 | +2.39 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4, Cuntze (FMC) | unidirectional | 36.33 | 37.186 | +2.36 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5, Tsai-Wu | unidirectional | 1376.4 | 1408.4 | +2.32 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 12, Tsai-Hill | unidirectional | 1249 | 1277.5 | +2.28 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9, Tsai-Wu | unidirectional | 114.55 | 112.04 | −2.19 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 6, Tsai-Wu | unidirectional | 1134.5 | 1112.2 | −1.96 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30, Max Stress | unidirectional | 565.09 | 575.16 | +1.78 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30, Max Strain | unidirectional | 565.09 | 575.16 | +1.78 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30, Hashin | unidirectional | 565.09 | 575.16 | +1.78 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30, Sun | unidirectional | 565.09 | 575.16 | +1.78 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 5, Cuntze (FMC) | unidirectional | 1041.4 | 1023.6 | −1.71 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6, Puck | unidirectional | 1481.3 | 1458 | −1.57 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 31, Tsai-Wu | unidirectional | 680.11 | 669.69 | −1.53 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3, Tsai-Hill | unidirectional | 44.562 | 45.231 | +1.50 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3, Hashin | unidirectional | 44.562 | 45.231 | +1.50 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3, Sun | unidirectional | 44.562 | 45.231 | +1.50 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3, Edge | unidirectional | 44.562 | 45.231 | +1.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4, Max Stress | unidirectional | 1522.9 | 1500.1 | −1.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4, Max Strain | unidirectional | 1522.9 | 1500.1 | −1.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4, Puck | unidirectional | 1522.9 | 1500.1 | −1.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4, Sun | unidirectional | 1522.9 | 1500.1 | −1.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 4, Edge | unidirectional | 1522.9 | 1500.1 | −1.50 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6, Max Stress | unidirectional | 1481.3 | 1500.8 | +1.31 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6, Max Strain | unidirectional | 1481.3 | 1500.8 | +1.31 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6, Sun | unidirectional | 1481.3 | 1500.8 | +1.31 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 6, Edge | unidirectional | 1481.3 | 1500.8 | +1.31 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2, Max Stress | unidirectional | 1481.1 | 1500 | +1.28 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2, Max Strain | unidirectional | 1481.1 | 1500 | +1.28 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2, Tsai-Hill | unidirectional | 1481.1 | 1500 | +1.28 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2, Tsai-Wu | unidirectional | 1481.1 | 1500 | +1.28 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2, Hashin | unidirectional | 1481.1 | 1500 | +1.28 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2, Puck | unidirectional | 1481.1 | 1500 | +1.28 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2, Cuntze (FMC) | unidirectional | 1481.1 | 1500 | +1.28 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2, Sun | unidirectional | 1481.1 | 1500 | +1.28 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 2, Edge | unidirectional | 1481.1 | 1500 | +1.28 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4, Tsai-Hill | unidirectional | 36.33 | 36.787 | +1.26 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4, Hashin | unidirectional | 36.33 | 36.787 | +1.26 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4, Sun | unidirectional | 36.33 | 36.787 | +1.26 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4, Edge | unidirectional | 36.33 | 36.787 | +1.26 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13, Tsai-Wu | unidirectional | 1200.7 | 1186 | −1.23 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 7, Puck | unidirectional | 1086.4 | 1099.1 | +1.17 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 9, Cuntze (FMC) | unidirectional | 1029.4 | 1018.5 | −1.06 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4, Puck | unidirectional | 36.33 | 36.706 | +1.04 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 20, Tsai-Wu | unidirectional | 246.84 | 244.95 | −0.77 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 17, Tsai-Wu | unidirectional | 838.84 | 832.74 | −0.73 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 21, Cuntze (FMC) | unidirectional | 791.48 | 797.1 | +0.71 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9, Sun | unidirectional | 114.55 | 115.31 | +0.66 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 11, Tsai-Wu | unidirectional | 1124.5 | 1118.3 | −0.55 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 14, Puck | unidirectional | 93.018 | 93.52 | +0.54 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 4, Tsai-Wu | unidirectional | 36.33 | 36.481 | +0.42 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5, Tsai-Hill | unidirectional | 1376.4 | 1382.1 | +0.41 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 5, Hashin | unidirectional | 1376.4 | 1382.1 | +0.41 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 30, Puck | unidirectional | 565.09 | 562.76 | −0.41 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 13, Tsai-Hill | unidirectional | 1200.7 | 1204.6 | +0.32 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 22, Tsai-Hill | unidirectional | 799.58 | 797.14 | −0.30 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 3, Puck | unidirectional | 44.562 | 44.642 | +0.18 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 14, Tsai-Hill | unidirectional | 1139.5 | 1141.3 | +0.15 % |
| WWFE-I E-glass/LY556 lamina σ2-τ12, point 9, Puck | unidirectional | 114.55 | 114.39 | −0.14 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3, Max Stress | unidirectional | 1500.7 | 1500 | −0.047 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3, Max Strain | unidirectional | 1500.7 | 1500 | −0.047 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3, Tsai-Hill | unidirectional | 1500.7 | 1500 | −0.047 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3, Tsai-Wu | unidirectional | 1500.7 | 1500 | −0.047 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3, Hashin | unidirectional | 1500.7 | 1500 | −0.047 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3, Puck | unidirectional | 1500.7 | 1500 | −0.047 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3, Cuntze (FMC) | unidirectional | 1500.7 | 1500 | −0.047 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3, Sun | unidirectional | 1500.7 | 1500 | −0.047 % |
| WWFE-I T300/BSL914C lamina σ1-τ12, point 3, Edge | unidirectional | 1500.7 | 1500 | −0.047 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1, Max Stress | unidirectional | 40 | 40 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1, Max Strain | unidirectional | 40 | 40 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1, Tsai-Hill | unidirectional | 40 | 40 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1, Tsai-Wu | unidirectional | 40 | 40 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1, Hashin | unidirectional | 40 | 40 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1, Puck | unidirectional | 40 | 40 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1, Cuntze (FMC) | unidirectional | 40 | 40 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1, Sun | unidirectional | 40 | 40 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 1, Edge | unidirectional | 40 | 40 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2, Max Stress | unidirectional | 1280 | 1280 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2, Max Strain | unidirectional | 1280 | 1280 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2, Tsai-Hill | unidirectional | 1280 | 1280 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2, Tsai-Wu | unidirectional | 1280 | 1280 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2, Hashin | unidirectional | 1280 | 1280 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2, Puck | unidirectional | 1280 | 1280 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2, Cuntze (FMC) | unidirectional | 1280 | 1280 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2, Sun | unidirectional | 1280 | 1280 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 2, Edge | unidirectional | 1280 | 1280 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3, Max Stress | unidirectional | 800 | 800 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3, Tsai-Hill | unidirectional | 800 | 800 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3, Tsai-Wu | unidirectional | 800 | 800 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3, Hashin | unidirectional | 800 | 800 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3, Puck | unidirectional | 800 | 800 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3, Cuntze (FMC) | unidirectional | 800 | 800 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3, Sun | unidirectional | 800 | 800 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 3, Edge | unidirectional | 800 | 800 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21, Max Stress | unidirectional | 145 | 145 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21, Max Strain | unidirectional | 145 | 145 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21, Tsai-Hill | unidirectional | 145 | 145 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21, Tsai-Wu | unidirectional | 145 | 145 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21, Hashin | unidirectional | 145 | 145 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21, Puck | unidirectional | 145 | 145 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21, Cuntze (FMC) | unidirectional | 145 | 145 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21, Sun | unidirectional | 145 | 145 | <0.001 % |
| WWFE-I E-glass/MY750 lamina σ1-σ2, point 21, Edge | unidirectional | 145 | 145 | <0.001 % |
Lovejoy, A. E., Scotti, S. J., Miller, S. G., Heimann, P. & Miller, S. S., "Characterization of IM7/8552 Thin-ply and Hybrid Thin-ply Composites", AIAA SciTech 2019, NTRS 20200002400.
Measured [ksi]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| IM7/8552 30 gsm hybrid unnotched compression unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 141.7 | 190.98 | +34.8 % | Known gap |
| IM7/8552 70 gsm hybrid unnotched compression unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 134.2 | 166.04 | +23.7 % | Known gap |
| IM7/8552 30 gsm quasi-isotropic unnotched compression unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 118.1 | 94.167 | −20.3 % | Known gap |
| IM7/8552 70 gsm quasi-isotropic unnotched compression unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 114.1 | 92.946 | −18.5 % | Over 10 % |
| IM7/8552 70 gsm hybrid unnotched tension unnotched strength [ksi], Puck | 201.5 | 230.68 | +14.5 % | Over 10 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 135.2 | 120.63 | −10.8 % | Over 10 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 137.9 | 128.65 | −6.70 % | Within 10 % |
| IM7/8552 30 gsm hybrid unnotched tension unnotched strength [ksi], Puck | 259.3 | 271.18 | +4.58 % | Within 10 % |
How to reproduce it
Source
Lovejoy, A. E., Scotti, S. J., Miller, S. G., Heimann, P. & Miller, S. S., "Characterization of IM7/8552 Thin-ply and Hybrid Thin-ply Composites", AIAA SciTech 2019, NTRS 20200002400.
Tables 3 and 4 (laminate); lamina Tables 3, 4 and 7
What was taken from it
The average unnotched tension and compression strength of the 30 and 70 gsm quasi-isotropic and hybrid laminates, with the lamina strengths of each grade.
Quantity compared: unnotched strength [ksi]
Inputs
- Lamina strengths per grade: XT and YT from Table 3, XC and YC from Table 4, S12 at 5 % shear strain from Table 7.
- Hybrids have thin ±45 plies and standard 190 gsm 0 and 90 plies. The standard plies take the NCAMP rows the paper prints.
- The quasi-isotropic layups run as [45/0/-45/90]s. Under in-plane load, every ply of one angle carries the same stress in a symmetric stack of repeated sublaminates.
- Uniaxial σ<sub>x</sub>, last-ply failure of the progressive failure tool.
- Every failure criterion the app has is a sub-case of each test, run with the app's default parameters. Nothing is tuned to the test and no cure residual stress is applied.
The inputs of each configuration are listed in the table below.
Allowed difference
±20 %; outside it, known gap
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| IM7/8552 30 gsm hybrid unnotched compression, Tsai-Wu | angle-ply | 141.7 | 214.05 | +51.1 % |
| IM7/8552 30 gsm hybrid unnotched compression, Tsai-Hill | angle-ply | 141.7 | 191.43 | +35.1 % |
| IM7/8552 30 gsm hybrid unnotched compression, Max Strain | angle-ply | 141.7 | 191.39 | +35.1 % |
| IM7/8552 30 gsm hybrid unnotched compression, Max Stress | angle-ply | 141.7 | 190.98 | +34.8 % |
| IM7/8552 30 gsm hybrid unnotched compression, Hashin | angle-ply | 141.7 | 190.98 | +34.8 % |
| IM7/8552 30 gsm hybrid unnotched compression, Puck | angle-ply | 141.7 | 190.98 | +34.8 % |
| IM7/8552 30 gsm hybrid unnotched compression, Sun | angle-ply | 141.7 | 190.98 | +34.8 % |
| IM7/8552 30 gsm hybrid unnotched compression, Cuntze (FMC) | angle-ply | 141.7 | 190.96 | +34.8 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension, Tsai-Wu | quasi-isotropic | 135.2 | 90.5 | −33.1 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension, Tsai-Hill | quasi-isotropic | 135.2 | 90.5 | −33.1 % |
| IM7/8552 30 gsm quasi-isotropic unnotched compression, Edge | quasi-isotropic | 118.1 | 81.867 | −30.7 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension, Tsai-Wu | quasi-isotropic | 137.9 | 96.525 | −30.0 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension, Tsai-Hill | quasi-isotropic | 137.9 | 96.525 | −30.0 % |
| IM7/8552 30 gsm hybrid unnotched compression, Edge | angle-ply | 141.7 | 183.39 | +29.4 % |
| IM7/8552 70 gsm quasi-isotropic unnotched compression, Edge | quasi-isotropic | 114.1 | 83.002 | −27.3 % |
| IM7/8552 70 gsm hybrid unnotched compression, Max Stress | angle-ply | 134.2 | 166.04 | +23.7 % |
| IM7/8552 70 gsm hybrid unnotched compression, Hashin | angle-ply | 134.2 | 166.04 | +23.7 % |
| IM7/8552 70 gsm hybrid unnotched compression, Puck | angle-ply | 134.2 | 166.04 | +23.7 % |
| IM7/8552 70 gsm hybrid unnotched compression, Sun | angle-ply | 134.2 | 166.04 | +23.7 % |
| IM7/8552 70 gsm hybrid unnotched compression, Cuntze (FMC) | angle-ply | 134.2 | 166 | +23.7 % |
| IM7/8552 70 gsm hybrid unnotched compression, Max Strain | angle-ply | 134.2 | 165.92 | +23.6 % |
| IM7/8552 70 gsm hybrid unnotched compression, Tsai-Hill | angle-ply | 134.2 | 165.63 | +23.4 % |
| IM7/8552 30 gsm quasi-isotropic unnotched compression, Cuntze (FMC) | quasi-isotropic | 118.1 | 94.164 | −20.3 % |
| IM7/8552 30 gsm quasi-isotropic unnotched compression, Max Stress | quasi-isotropic | 118.1 | 94.167 | −20.3 % |
| IM7/8552 30 gsm quasi-isotropic unnotched compression, Hashin | quasi-isotropic | 118.1 | 94.167 | −20.3 % |
| IM7/8552 30 gsm quasi-isotropic unnotched compression, Puck | quasi-isotropic | 118.1 | 94.167 | −20.3 % |
| IM7/8552 30 gsm quasi-isotropic unnotched compression, Sun | quasi-isotropic | 118.1 | 94.167 | −20.3 % |
| IM7/8552 30 gsm quasi-isotropic unnotched compression, Max Strain | quasi-isotropic | 118.1 | 94.289 | −20.2 % |
| IM7/8552 30 gsm quasi-isotropic unnotched compression, Tsai-Hill | quasi-isotropic | 118.1 | 94.31 | −20.1 % |
| IM7/8552 70 gsm hybrid unnotched compression, Tsai-Wu | angle-ply | 134.2 | 159.97 | +19.2 % |
| IM7/8552 70 gsm quasi-isotropic unnotched compression, Cuntze (FMC) | quasi-isotropic | 114.1 | 92.944 | −18.5 % |
| IM7/8552 70 gsm quasi-isotropic unnotched compression, Max Stress | quasi-isotropic | 114.1 | 92.946 | −18.5 % |
| IM7/8552 70 gsm quasi-isotropic unnotched compression, Hashin | quasi-isotropic | 114.1 | 92.946 | −18.5 % |
| IM7/8552 70 gsm quasi-isotropic unnotched compression, Puck | quasi-isotropic | 114.1 | 92.946 | −18.5 % |
| IM7/8552 70 gsm quasi-isotropic unnotched compression, Sun | quasi-isotropic | 114.1 | 92.946 | −18.5 % |
| IM7/8552 70 gsm quasi-isotropic unnotched compression, Max Strain | quasi-isotropic | 114.1 | 93.069 | −18.4 % |
| IM7/8552 70 gsm quasi-isotropic unnotched compression, Tsai-Hill | quasi-isotropic | 114.1 | 93.093 | −18.4 % |
| IM7/8552 70 gsm hybrid unnotched tension, Max Stress | angle-ply | 201.5 | 234.05 | +16.2 % |
| IM7/8552 70 gsm hybrid unnotched tension, Max Strain | angle-ply | 201.5 | 234.05 | +16.2 % |
| IM7/8552 30 gsm quasi-isotropic unnotched compression, Tsai-Wu | quasi-isotropic | 118.1 | 99.947 | −15.4 % |
| IM7/8552 70 gsm hybrid unnotched tension, Hashin | angle-ply | 201.5 | 230.68 | +14.5 % |
| IM7/8552 70 gsm hybrid unnotched tension, Puck | angle-ply | 201.5 | 230.68 | +14.5 % |
| IM7/8552 70 gsm hybrid unnotched tension, Sun | angle-ply | 201.5 | 230.68 | +14.5 % |
| IM7/8552 70 gsm hybrid unnotched tension, Edge | angle-ply | 201.5 | 230.68 | +14.5 % |
| IM7/8552 70 gsm hybrid unnotched tension, Cuntze (FMC) | angle-ply | 201.5 | 230.64 | +14.5 % |
| IM7/8552 70 gsm hybrid unnotched compression, Edge | angle-ply | 134.2 | 153.55 | +14.4 % |
| IM7/8552 70 gsm quasi-isotropic unnotched compression, Tsai-Wu | quasi-isotropic | 114.1 | 97.881 | −14.2 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension, Cuntze (FMC) | quasi-isotropic | 135.2 | 120.62 | −10.8 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension, Hashin | quasi-isotropic | 135.2 | 120.63 | −10.8 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension, Puck | quasi-isotropic | 135.2 | 120.63 | −10.8 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension, Sun | quasi-isotropic | 135.2 | 120.63 | −10.8 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension, Edge | quasi-isotropic | 135.2 | 120.63 | −10.8 % |
| IM7/8552 70 gsm hybrid unnotched tension, Tsai-Wu | angle-ply | 201.5 | 215.23 | +6.81 % |
| IM7/8552 70 gsm hybrid unnotched tension, Tsai-Hill | angle-ply | 201.5 | 215.23 | +6.81 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension, Cuntze (FMC) | quasi-isotropic | 137.9 | 128.64 | −6.72 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension, Max Stress | quasi-isotropic | 137.9 | 128.65 | −6.70 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension, Hashin | quasi-isotropic | 137.9 | 128.65 | −6.70 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension, Puck | quasi-isotropic | 137.9 | 128.65 | −6.70 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension, Sun | quasi-isotropic | 137.9 | 128.65 | −6.70 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension, Edge | quasi-isotropic | 137.9 | 128.65 | −6.70 % |
| IM7/8552 30 gsm quasi-isotropic unnotched tension, Max Strain | quasi-isotropic | 137.9 | 128.7 | −6.67 % |
| IM7/8552 30 gsm hybrid unnotched tension, Max Strain | angle-ply | 259.3 | 275.24 | +6.15 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension, Max Stress | quasi-isotropic | 135.2 | 127.18 | −5.93 % |
| IM7/8552 70 gsm quasi-isotropic unnotched tension, Max Strain | quasi-isotropic | 135.2 | 127.18 | −5.93 % |
| IM7/8552 30 gsm hybrid unnotched tension, Max Stress | angle-ply | 259.3 | 271.18 | +4.58 % |
| IM7/8552 30 gsm hybrid unnotched tension, Hashin | angle-ply | 259.3 | 271.18 | +4.58 % |
| IM7/8552 30 gsm hybrid unnotched tension, Puck | angle-ply | 259.3 | 271.18 | +4.58 % |
| IM7/8552 30 gsm hybrid unnotched tension, Sun | angle-ply | 259.3 | 271.18 | +4.58 % |
| IM7/8552 30 gsm hybrid unnotched tension, Edge | angle-ply | 259.3 | 271.18 | +4.58 % |
| IM7/8552 30 gsm hybrid unnotched tension, Cuntze (FMC) | angle-ply | 259.3 | 270.37 | +4.27 % |
| IM7/8552 30 gsm hybrid unnotched tension, Tsai-Hill | angle-ply | 259.3 | 261.14 | +0.71 % |
| IM7/8552 30 gsm hybrid unnotched tension, Tsai-Wu | angle-ply | 259.3 | 261.14 | +0.71 % |
NCAMP, "Hexcel 8552 IM7 Unidirectional Prepreg 190 gsm & 35%RC Qualification Statistical Analysis Report", NCP-RP-2009-028 Rev B, April 16, 2019. Stacking sequences from the Material Property Data Report CAM-RP-2009-015 Rev B, April 16, 2019.
Measured [ksi]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 79.42 | 98.927 | +24.6 % | Known gap |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 120.84 | 146.74 | +21.4 % | Known gap |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 99.35 | 119.28 | +20.1 % | Known gap |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 54.17 | 43.515 | −19.7 % | Over 10 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD unnotched strength [ksi], Puck | 152.58 | 178.7 | +17.1 % | Over 10 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD unnotched strength [ksi], Puck | 104.69 | 120.93 | +15.5 % | Over 10 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD unnotched strength [ksi], Puck | 175.63 | 200.37 | +14.1 % | Over 10 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 70.22 | 60.334 | −14.1 % | Over 10 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD unnotched strength [ksi], Puck | 174.18 | 197.78 | +13.5 % | Over 10 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 40.61 | 35.61 | −12.3 % | Over 10 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD unnotched strength [ksi], Puck | 87.05 | 95.621 | +9.85 % | Within 10 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW unnotched strength [ksi], Puck | 57.68 | 62.947 | +9.13 % | Within 10 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 67.01 | 61.075 | −8.86 % | Within 10 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 66.44 | 61.573 | −7.33 % | Within 10 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW unnotched strength [ksi], Puck | 179.23 | 166.75 | −6.96 % | Within 10 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD unnotched strength [ksi], Puck | 171.38 | 181.35 | +5.81 % | Within 10 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW unnotched strength [ksi], Puck | 187.43 | 183.73 | −1.98 % | Within 10 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW unnotched strength [ksi], PuckWhy: At least one failure criterion falls outside the band for this test. The tools run on the lamina strengths the source printed, with the app’s default criterion parameters and no cure residual stress, and nothing is tuned to the test. | 112.46 | 111.09 | −1.22 % | Within 10 % |
How to reproduce it
Source
NCAMP, "Hexcel 8552 IM7 Unidirectional Prepreg 190 gsm & 35%RC Qualification Statistical Analysis Report", NCP-RP-2009-028 Rev B, April 16, 2019. Stacking sequences from the Material Property Data Report CAM-RP-2009-015 Rev B, April 16, 2019.
Tables 4-3 to 4-13 (lamina) and 5-1 to 5-11 (laminate)
What was taken from it
The normalized mean unnotched strengths of the quasi-isotropic, soft, hard and cross-ply laminates at CTD, RTD and ETW, with the lamina strengths of the same report.
Quantity compared: unnotched strength [ksi]
Inputs
- Lamina strengths per environment: F1tu from the 0° tension test, F1cu backed out of the UNC0 test (the report prints no direct 0° compression strength), F2tu, F2cu, and F12 at 5 % shear strain. The CTD shear specimens failed before 5 %, so F12 there is their maximum stress.
- Tension laminates use the tension moduli and compression laminates the compression moduli.
- Uniaxial σ<sub>x</sub>, last-ply failure of the progressive failure tool. Compression was tested at RTD and ETW only.
- Every failure criterion the app has is a sub-case of each test, run with the app's default parameters. Nothing is tuned to the test and no cure residual stress is applied.
The inputs of each configuration are listed in the table below.
Allowed difference
±20 %; outside it, known gap
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW, Tsai-Hill | angle-ply | 54.17 | 33.35 | −38.4 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW, Tsai-Wu | angle-ply | 54.17 | 33.35 | −38.4 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD, Tsai-Wu | angle-ply | 67.01 | 43.487 | −35.1 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD, Tsai-Wu | angle-ply | 70.22 | 46.625 | −33.6 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD, Tsai-Hill | angle-ply | 67.01 | 45.459 | −32.2 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD, Tsai-Hill | angle-ply | 70.22 | 49.953 | −28.9 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD, Tsai-Wu | angle-ply | 66.44 | 47.381 | −28.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW, Tsai-Hill | angle-ply | 40.61 | 29.018 | −28.5 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD, Max Strain | quasi-isotropic | 99.35 | 125.3 | +26.1 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW, Tsai-Wu | quasi-isotropic | 112.46 | 83.375 | −25.9 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW, Tsai-Hill | quasi-isotropic | 112.46 | 83.375 | −25.9 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW, Tsai-Wu | angle-ply | 40.61 | 30.164 | −25.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD, Edge | angle-ply | 66.44 | 50.002 | −24.7 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW, Max Stress | angle-ply | 79.42 | 98.927 | +24.6 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW, Hashin | angle-ply | 79.42 | 98.927 | +24.6 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW, Puck | angle-ply | 79.42 | 98.927 | +24.6 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW, Sun | angle-ply | 79.42 | 98.927 | +24.6 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW, Edge | angle-ply | 79.42 | 98.927 | +24.6 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW, Max Strain | angle-ply | 79.42 | 98.661 | +24.2 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD, Max Stress | quasi-isotropic | 99.35 | 122.25 | +23.1 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW, Cuntze (FMC) | angle-ply | 79.42 | 97.344 | +22.6 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD, Max Stress | angle-ply | 120.84 | 146.74 | +21.4 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD, Hashin | angle-ply | 120.84 | 146.74 | +21.4 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD, Puck | angle-ply | 120.84 | 146.74 | +21.4 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD, Sun | angle-ply | 120.84 | 146.74 | +21.4 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD, Max Strain | angle-ply | 120.84 | 146.44 | +21.2 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD, Cuntze (FMC) | angle-ply | 120.84 | 146.21 | +21.0 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD, Hashin | quasi-isotropic | 99.35 | 119.28 | +20.1 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD, Puck | quasi-isotropic | 99.35 | 119.28 | +20.1 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD, Sun | quasi-isotropic | 99.35 | 119.28 | +20.1 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD, Edge | quasi-isotropic | 99.35 | 119.28 | +20.1 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD, Cuntze (FMC) | quasi-isotropic | 99.35 | 119.27 | +20.1 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD, Tsai-Hill | angle-ply | 120.84 | 144.66 | +19.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW, Hashin | angle-ply | 54.17 | 43.515 | −19.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW, Puck | angle-ply | 54.17 | 43.515 | −19.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW, Sun | angle-ply | 54.17 | 43.515 | −19.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW, Edge | angle-ply | 54.17 | 43.515 | −19.7 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW, Tsai-Hill | angle-ply | 79.42 | 95.037 | +19.7 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD, Max Stress | quasi-isotropic | 104.69 | 124.92 | +19.3 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD, Max Strain | quasi-isotropic | 104.69 | 124.92 | +19.3 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW, Tsai-Wu | quasi-isotropic | 57.68 | 68.398 | +18.6 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD, Max Strain | cross-ply | 152.58 | 179.49 | +17.6 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD, Tsai-Hill | cross-ply | 152.58 | 178.7 | +17.1 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD, Puck | cross-ply | 152.58 | 178.7 | +17.1 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD, Max Stress | cross-ply | 152.58 | 178.7 | +17.1 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD, Hashin | cross-ply | 152.58 | 178.7 | +17.1 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD, Sun | cross-ply | 152.58 | 178.7 | +17.1 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD, Edge | cross-ply | 152.58 | 178.7 | +17.1 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD, Tsai-Wu | cross-ply | 152.58 | 178.69 | +17.1 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW, Cuntze (FMC) | angle-ply | 54.17 | 45.637 | −15.8 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD, Hashin | quasi-isotropic | 104.69 | 120.93 | +15.5 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD, Puck | quasi-isotropic | 104.69 | 120.93 | +15.5 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD, Sun | quasi-isotropic | 104.69 | 120.93 | +15.5 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD, Edge | quasi-isotropic | 104.69 | 120.93 | +15.5 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD, Cuntze (FMC) | quasi-isotropic | 104.69 | 120.93 | +15.5 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD, Tsai-Wu | quasi-isotropic | 87.05 | 100.31 | +15.2 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD, Tsai-Hill | angle-ply | 66.44 | 56.82 | −14.5 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD, Max Stress | angle-ply | 175.63 | 200.37 | +14.1 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD, Hashin | angle-ply | 175.63 | 200.37 | +14.1 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD, Puck | angle-ply | 175.63 | 200.37 | +14.1 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD, Sun | angle-ply | 175.63 | 200.37 | +14.1 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD, Edge | angle-ply | 175.63 | 200.37 | +14.1 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD, Puck | angle-ply | 70.22 | 60.334 | −14.1 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD, Cuntze (FMC) | angle-ply | 175.63 | 200.22 | +14.0 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW, Cuntze (FMC) | angle-ply | 40.61 | 35.01 | −13.8 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD, Max Strain | angle-ply | 175.63 | 199.79 | +13.8 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD, Max Stress | angle-ply | 174.18 | 197.78 | +13.5 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD, Hashin | angle-ply | 174.18 | 197.78 | +13.5 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD, Puck | angle-ply | 174.18 | 197.78 | +13.5 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD, Sun | angle-ply | 174.18 | 197.78 | +13.5 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD, Edge | angle-ply | 174.18 | 197.78 | +13.5 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD, Cuntze (FMC) | angle-ply | 174.18 | 197.62 | +13.5 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD, Tsai-Wu | quasi-isotropic | 104.69 | 90.673 | −13.4 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, RTD, Tsai-Hill | quasi-isotropic | 104.69 | 90.673 | −13.4 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD, Max Strain | angle-ply | 174.18 | 197.09 | +13.2 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD, Hashin | angle-ply | 70.22 | 61.278 | −12.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD, Sun | angle-ply | 70.22 | 61.278 | −12.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD, Edge | angle-ply | 70.22 | 61.278 | −12.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW, Max Strain | angle-ply | 40.61 | 35.61 | −12.3 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW, Puck | angle-ply | 40.61 | 35.61 | −12.3 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW, Max Stress | angle-ply | 40.61 | 35.869 | −11.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW, Hashin | angle-ply | 40.61 | 35.869 | −11.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW, Sun | angle-ply | 40.61 | 35.869 | −11.7 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, ETW, Edge | angle-ply | 40.61 | 35.869 | −11.7 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW, Tsai-Hill | angle-ply | 187.43 | 166.75 | −11.0 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW, Tsai-Wu | angle-ply | 187.43 | 166.75 | −11.0 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD, Cuntze (FMC) | angle-ply | 66.44 | 59.254 | −10.8 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD, Tsai-Hill | quasi-isotropic | 99.35 | 89.348 | −10.1 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, CTD, Tsai-Wu | quasi-isotropic | 99.35 | 89.348 | −10.1 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD, Tsai-Hill | quasi-isotropic | 87.05 | 95.733 | +9.97 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD, Max Strain | quasi-isotropic | 87.05 | 95.709 | +9.95 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD, Max Stress | quasi-isotropic | 87.05 | 95.621 | +9.85 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD, Hashin | quasi-isotropic | 87.05 | 95.621 | +9.85 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD, Puck | quasi-isotropic | 87.05 | 95.621 | +9.85 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD, Sun | quasi-isotropic | 87.05 | 95.621 | +9.85 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD, Cuntze (FMC) | quasi-isotropic | 87.05 | 95.62 | +9.85 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD, Tsai-Wu | angle-ply | 120.84 | 132.3 | +9.48 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW, Tsai-Hill | quasi-isotropic | 57.68 | 63.004 | +9.23 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW, Max Strain | quasi-isotropic | 57.68 | 63.001 | +9.22 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW, Max Stress | quasi-isotropic | 57.68 | 62.947 | +9.13 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW, Hashin | quasi-isotropic | 57.68 | 62.947 | +9.13 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW, Puck | quasi-isotropic | 57.68 | 62.947 | +9.13 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW, Sun | quasi-isotropic | 57.68 | 62.947 | +9.13 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW, Edge | quasi-isotropic | 57.68 | 62.947 | +9.13 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, ETW, Cuntze (FMC) | quasi-isotropic | 57.68 | 62.945 | +9.13 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD, Hashin | angle-ply | 67.01 | 61.075 | −8.86 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD, Puck | angle-ply | 67.01 | 61.075 | −8.86 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD, Sun | angle-ply | 67.01 | 61.075 | −8.86 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD, Edge | angle-ply | 67.01 | 61.075 | −8.86 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, RTD, Edge | angle-ply | 120.84 | 131.37 | +8.71 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD, Hashin | angle-ply | 66.44 | 60.78 | −8.52 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD, Cuntze (FMC) | angle-ply | 70.22 | 64.254 | −8.50 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD, Max Strain | angle-ply | 66.44 | 61.017 | −8.16 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched compression, RTD, Edge | quasi-isotropic | 87.05 | 80.087 | −8.00 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD, Cuntze (FMC) | angle-ply | 67.01 | 61.732 | −7.88 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD, Max Stress | angle-ply | 66.44 | 61.259 | −7.80 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD, Puck | angle-ply | 66.44 | 61.573 | −7.33 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched compression, RTD, Sun | angle-ply | 66.44 | 61.573 | −7.33 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW, Tsai-Wu | cross-ply | 179.23 | 166.75 | −6.96 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW, Cuntze (FMC) | cross-ply | 179.23 | 166.75 | −6.96 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW, Max Stress | cross-ply | 179.23 | 166.75 | −6.96 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW, Hashin | cross-ply | 179.23 | 166.75 | −6.96 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW, Puck | cross-ply | 179.23 | 166.75 | −6.96 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW, Sun | cross-ply | 179.23 | 166.75 | −6.96 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW, Edge | cross-ply | 179.23 | 166.75 | −6.96 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW, Tsai-Hill | cross-ply | 179.23 | 166.75 | −6.96 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, ETW, Max Strain | cross-ply | 179.23 | 167.6 | −6.49 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD, Max Strain | cross-ply | 171.38 | 182.32 | +6.38 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD, Cuntze (FMC) | cross-ply | 171.38 | 160.63 | −6.27 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD, Tsai-Hill | cross-ply | 171.38 | 181.35 | +5.81 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD, Puck | cross-ply | 171.38 | 181.35 | +5.81 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD, Max Stress | cross-ply | 171.38 | 181.35 | +5.81 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD, Hashin | cross-ply | 171.38 | 181.35 | +5.81 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD, Sun | cross-ply | 171.38 | 181.35 | +5.81 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD, Edge | cross-ply | 171.38 | 181.35 | +5.81 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, RTD, Tsai-Wu | cross-ply | 171.38 | 181.34 | +5.81 % |
| NCAMP 8552 IM7 cross-ply UNT0 unnotched tension, CTD, Cuntze (FMC) | cross-ply | 152.58 | 161.32 | +5.73 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW, Max Stress | angle-ply | 54.17 | 51.88 | −4.23 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, ETW, Max Strain | angle-ply | 54.17 | 51.88 | −4.23 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD, Tsai-Wu | angle-ply | 175.63 | 181.35 | +3.25 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, RTD, Tsai-Hill | angle-ply | 175.63 | 181.35 | +3.25 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD, Tsai-Wu | angle-ply | 174.18 | 178.7 | +2.59 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, CTD, Tsai-Hill | angle-ply | 174.18 | 178.7 | +2.59 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched compression, ETW, Tsai-Wu | angle-ply | 79.42 | 81.245 | +2.30 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW, Max Strain | angle-ply | 187.43 | 183.48 | −2.10 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW, Cuntze (FMC) | angle-ply | 187.43 | 183.66 | −2.01 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW, Max Stress | angle-ply | 187.43 | 183.73 | −1.98 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW, Hashin | angle-ply | 187.43 | 183.73 | −1.98 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW, Puck | angle-ply | 187.43 | 183.73 | −1.98 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW, Sun | angle-ply | 187.43 | 183.73 | −1.98 % |
| NCAMP 8552 IM7 hard 50/40/10 unnotched tension, ETW, Edge | angle-ply | 187.43 | 183.73 | −1.98 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW, Cuntze (FMC) | quasi-isotropic | 112.46 | 110.41 | −1.83 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD, Max Stress | angle-ply | 67.01 | 66.126 | −1.32 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, RTD, Max Strain | angle-ply | 67.01 | 66.126 | −1.32 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW, Max Stress | quasi-isotropic | 112.46 | 111.09 | −1.22 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW, Hashin | quasi-isotropic | 112.46 | 111.09 | −1.22 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW, Puck | quasi-isotropic | 112.46 | 111.09 | −1.22 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW, Sun | quasi-isotropic | 112.46 | 111.09 | −1.22 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW, Edge | quasi-isotropic | 112.46 | 111.09 | −1.22 % |
| NCAMP 8552 IM7 quasi-isotropic 25/50/25 unnotched tension, ETW, Max Strain | quasi-isotropic | 112.46 | 111.18 | −1.14 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD, Max Stress | angle-ply | 70.22 | 70.315 | +0.13 % |
| NCAMP 8552 IM7 soft 10/80/10 unnotched tension, CTD, Max Strain | angle-ply | 70.22 | 70.315 | +0.13 % |
Jones, R. M., Mechanics of Composite Materials, 2nd Ed., Taylor and Francis (1999).
Largest error against the reference for each configuration, worst first. The axis is logarithmic: each step up is ten times the error.
4 configurations, largest error first
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Single ply, closed form: [0°] single ply, uniaxial Nx = S1t × h = 187.5 N/mm → σ1 = S1t → FI = 1.0 (all criteria) ply stress [MPa], failure index [-], safety factor [-], σ₂ | 0 | -3.7246 × 10⁻¹⁵ | <0.001 % | Within 1 % |
| Single ply, closed form: [90°] single ply, Nx = S2t × h = 5.0 N/mm → σ2 = S2t = 40 MPa → FI = 1.0 (all criteria) ply stress [MPa], failure index [-], safety factor [-], σ₁ | 0 | -2.3718 × 10⁻¹⁵ | <0.001 % | Within 1 % |
| Single ply, closed form: [0°] single ply at 50% of failure load: Nx = 93.75 N/mm → σ1 = 750 MPa = S1t/2 → safety factor = 2.0 ply stress [MPa], failure index [-], safety factor [-], σ₂ | 0 | -1.8623 × 10⁻¹⁵ | <0.001 % | Within 1 % |
| Single ply, closed form: [90°] single ply at 50% of failure load: Nx = 2.5 N/mm → σ2 = 20 MPa = S2t/2 → safety factor = 2.0 ply stress [MPa], failure index [-], safety factor [-], σ₁ | 0 | -2.7684 × 10⁻¹⁶ | <0.001 % | Within 1 % |
How to reproduce it
Source
Jones, R. M., Mechanics of Composite Materials, 2nd Ed., Taylor and Francis (1999).
Chapter 4 and Sections 2.6, 2.9
What was taken from it
The failure index definitions. A single ply loaded to its strength must give an index of 1, and half that load a safety factor of 2.
Quantity compared: ply stress [MPa], failure index [-], safety factor [-]
Inputs
The inputs of each configuration are listed in the table below.
Allowed difference
per sub-case, below
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Single ply, closed form: [0°] single ply, uniaxial Nx = S1t × h = 187.5 N/mm → σ1 = S1t → FI = 1.0 (all criteria), σ₂ | unidirectional | 0 | -3.7246 × 10⁻¹⁵ | <0.001 % |
| Single ply, closed form: [90°] single ply, Nx = S2t × h = 5.0 N/mm → σ2 = S2t = 40 MPa → FI = 1.0 (all criteria), σ₁ | unidirectional | 0 | -2.3718 × 10⁻¹⁵ | <0.001 % |
| Single ply, closed form: [0°] single ply at 50% of failure load: Nx = 93.75 N/mm → σ1 = 750 MPa = S1t/2 → safety factor = 2.0, σ₂ | unidirectional | 0 | -1.8623 × 10⁻¹⁵ | <0.001 % |
| Single ply, closed form: [90°] single ply at 50% of failure load: Nx = 2.5 N/mm → σ2 = 20 MPa = S2t/2 → safety factor = 2.0, σ₁ | unidirectional | 0 | -2.7684 × 10⁻¹⁶ | <0.001 % |
| Single ply, closed form: [0°] single ply at 50% of failure load: Nx = 93.75 N/mm → σ1 = 750 MPa = S1t/2 → safety factor = 2.0, Tsai-Wu FI | unidirectional | 0.25 | 0.25 | <0.001 % |
| Single ply, closed form: [0°] single ply, uniaxial Nx = S1t × h = 187.5 N/mm → σ1 = S1t → FI = 1.0 (all criteria), σ₁ | unidirectional | 1500 | 1500 | <0.001 % |
| Single ply, closed form: [0°] single ply, uniaxial Nx = S1t × h = 187.5 N/mm → σ1 = S1t → FI = 1.0 (all criteria), τ₁₂ | unidirectional | 0 | 0 | <0.001 % |
| Single ply, closed form: [0°] single ply, uniaxial Nx = S1t × h = 187.5 N/mm → σ1 = S1t → FI = 1.0 (all criteria), Max Stress FI | unidirectional | 1 | 1 | <0.001 % |
| Single ply, closed form: [0°] single ply, uniaxial Nx = S1t × h = 187.5 N/mm → σ1 = S1t → FI = 1.0 (all criteria), Tsai-Hill FI | unidirectional | 1 | 1 | <0.001 % |
| Single ply, closed form: [0°] single ply, uniaxial Nx = S1t × h = 187.5 N/mm → σ1 = S1t → FI = 1.0 (all criteria), Tsai-Wu FI | unidirectional | 1 | 1 | <0.001 % |
| Single ply, closed form: [0°] single ply, uniaxial Nx = S1t × h = 187.5 N/mm → σ1 = S1t → FI = 1.0 (all criteria), Safety factor | unidirectional | 1 | 1 | <0.001 % |
| Single ply, closed form: [90°] single ply, Nx = S2t × h = 5.0 N/mm → σ2 = S2t = 40 MPa → FI = 1.0 (all criteria), σ₂ | unidirectional | 40 | 40 | <0.001 % |
| Single ply, closed form: [90°] single ply, Nx = S2t × h = 5.0 N/mm → σ2 = S2t = 40 MPa → FI = 1.0 (all criteria), τ₁₂ | unidirectional | 0 | 0 | <0.001 % |
| Single ply, closed form: [90°] single ply, Nx = S2t × h = 5.0 N/mm → σ2 = S2t = 40 MPa → FI = 1.0 (all criteria), Max Stress FI | unidirectional | 1 | 1 | <0.001 % |
| Single ply, closed form: [90°] single ply, Nx = S2t × h = 5.0 N/mm → σ2 = S2t = 40 MPa → FI = 1.0 (all criteria), Tsai-Hill FI | unidirectional | 1 | 1 | <0.001 % |
| Single ply, closed form: [90°] single ply, Nx = S2t × h = 5.0 N/mm → σ2 = S2t = 40 MPa → FI = 1.0 (all criteria), Tsai-Wu FI | unidirectional | 1 | 1 | <0.001 % |
| Single ply, closed form: [90°] single ply, Nx = S2t × h = 5.0 N/mm → σ2 = S2t = 40 MPa → FI = 1.0 (all criteria), Safety factor | unidirectional | 1 | 1 | <0.001 % |
| Single ply, closed form: [0°] single ply at 50% of failure load: Nx = 93.75 N/mm → σ1 = 750 MPa = S1t/2 → safety factor = 2.0, σ₁ | unidirectional | 750 | 750 | <0.001 % |
| Single ply, closed form: [0°] single ply at 50% of failure load: Nx = 93.75 N/mm → σ1 = 750 MPa = S1t/2 → safety factor = 2.0, Max Stress FI | unidirectional | 0.5 | 0.5 | <0.001 % |
| Single ply, closed form: [0°] single ply at 50% of failure load: Nx = 93.75 N/mm → σ1 = 750 MPa = S1t/2 → safety factor = 2.0, Tsai-Hill FI | unidirectional | 0.25 | 0.25 | <0.001 % |
| Single ply, closed form: [0°] single ply at 50% of failure load: Nx = 93.75 N/mm → σ1 = 750 MPa = S1t/2 → safety factor = 2.0, Safety factor | unidirectional | 2 | 2 | <0.001 % |
| Single ply, closed form: [90°] single ply at 50% of failure load: Nx = 2.5 N/mm → σ2 = 20 MPa = S2t/2 → safety factor = 2.0, σ₂ | unidirectional | 20 | 20 | <0.001 % |
| Single ply, closed form: [90°] single ply at 50% of failure load: Nx = 2.5 N/mm → σ2 = 20 MPa = S2t/2 → safety factor = 2.0, Max Stress FI | unidirectional | 0.5 | 0.5 | <0.001 % |
| Single ply, closed form: [90°] single ply at 50% of failure load: Nx = 2.5 N/mm → σ2 = 20 MPa = S2t/2 → safety factor = 2.0, Tsai-Hill FI | unidirectional | 0.25 | 0.25 | <0.001 % |
| Single ply, closed form: [90°] single ply at 50% of failure load: Nx = 2.5 N/mm → σ2 = 20 MPa = S2t/2 → safety factor = 2.0, Tsai-Wu FI | unidirectional | 0.45935 | 0.45935 | <0.001 % |
| Single ply, closed form: [90°] single ply at 50% of failure load: Nx = 2.5 N/mm → σ2 = 20 MPa = S2t/2 → safety factor = 2.0, Safety factor | unidirectional | 2 | 2 | <0.001 % |
The tick on each bar marks the limit for that group. A bar past the tick is over the limit.
How the numbers are checked
The two groups answer two different questions. Reference solutions check that the program solves its equations correctly: the same model, solved by someone else in a published solution, an independent implementation or a finite element model, gives the same number. Engineers call this verification. Lab tests check that the equations describe a real part, which no amount of matching other programs can show. That is validation. A method can pass every verification case and still differ from a test, because the model leaves something out. The terms follow NAFEMS, What is Verification and Validation? (2014).
A reference case counts as within when its error is at most 1 %, a lab case when it is at most 10 %. A known gap is a case where the method and the reference disagree for a reason that is understood. It stays on this page with its reason until the method changes.