- Verification
- /
- Laminate and CLT
Laminate stiffness and CLT verification
Laminate stiffness, thermal resultants and spring-in from classical lamination theory, compared with lab tests and published results.
How close the results are
Lab tests show how close a prediction comes to a measured part. Reference solutions show that the program solves its equations the way someone else solved the same problem. A case is one configuration checked against one source, and it scores by its value with the largest error. A lab case that runs every failure criterion or every micromechanics model scores by Puck (the Puck failure criterion or the Puck micromechanics model), the same choice for all of them. The other models show in its row. Fitted cases show in their source but stay out of every number.
Lab tests: strength
Validation: failure loads of coupons, tubes, beams and joints, compared with published test programs. Where the app has several failure criteria, a case scores by Puck. The other criteria show in its row.
No lab test of this kind is published for laminate and clt yet.
Published solutions
Verification: the same inputs run against worked examples, tables and closed-form answers printed in textbooks, NASA reports and journal papers.
- Cases
- 4 cases from 1 source, 8 compared numbers
- Within 1 %
- 0 of 4
- Median error
- 1.18 %
- Largest error
- 1.27 %
- Known gaps
- None
Finite element models
Verification: a plane-stress finite element model of the same problem, solved in an open-source code. Each model runs on two meshes.
No finite element model is listed for laminate and clt yet.
ABD Composites runs no tests of its own. Each measured value comes from a published test program.
Sources
Each row is one source the results are checked against. Error is the difference between the program's value and the source's value, as a percentage of the source's value. A reference case passes at 1 % or less, a lab case at 10 % or less. Open a row to see every case, its chart and how to reproduce each number.
NCAMP, "Hexcel 8552 IM7 Unidirectional Prepreg 190 gsm & 35%RC Qualification Statistical Analysis Report", NCP-RP-2009-028 Rev B, April 16, 2019. Stacking sequences from the Material Property Data Report CAM-RP-2009-015 Rev B, April 16, 2019.
Measured
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Cross-ply compression, ETW modulus [Msi], Poisson's ratio, νxy compression Specimens: UNC0 8 specimens, coefficient of variation 3.04 % (SAR Table 4-16) Why: The measured Poisson's ratio is 0.017, so a difference of 0.015 is a large percentage. The modulus of the same specimens agrees. | 0.017 | 0.032343 | +90.3 % | Known gap |
| Hard, ETW modulus [Msi], Poisson's ratio, νxy compression Specimens: UNT3 22 specimens, coefficient of variation 4.65 %; UNC3 15 specimens, coefficient of variation 2.35 % (SAR Tables 5-6 and 5-12) Why: Hot and wet, the matrix softens and G12 drops to a third of its dry value. The predicted Poisson's ratio of this 0°-rich layup leans on that least certain lamina value. | 0.416 | 0.47917 | +15.2 % | Known gap |
| Quasi-isotropic, ETW modulus [Msi], Poisson's ratio, Ex tension Specimens: UNT1 17 specimens, coefficient of variation 5.16 %; UNC1 16 specimens, coefficient of variation 1.80 % (SAR Tables 5-2 and 5-8) | 7.99 | 8.5178 | +6.61 % | Within 10 % |
| Soft, ETW modulus [Msi], Poisson's ratio, Ex tension Specimens: UNT2 18 specimens, coefficient of variation 2.13 %; UNC2 16 specimens, coefficient of variation 2.21 % (SAR Tables 5-4 and 5-10) | 4.47 | 4.7625 | +6.54 % | Within 10 % |
| Cross-ply compression, CTD modulus [Msi], Poisson's ratio, νxy compression Specimens: UNC0 9 specimens, coefficient of variation 3.08 % (SAR Table 4-16) | 0.041 | 0.03874 | −5.51 % | Within 10 % |
| Cross-ply tension, ETW modulus [Msi], Poisson's ratio, Ex tension Specimens: UNT0 19 specimens, coefficient of variation 1.76 % (SAR Table 4-14) | 11.94 | 12.462 | +4.37 % | Within 10 % |
| Quasi-isotropic, CTD modulus [Msi], Poisson's ratio, Ex tension Specimens: UNT1 16 specimens, coefficient of variation 3.70 % (SAR Table 5-2) | 8.35 | 8.7144 | +4.36 % | Within 10 % |
| Quasi-isotropic, RTD modulus [Msi], Poisson's ratio, νxy compression Specimens: UNT1 16 specimens, coefficient of variation 5.73 %; UNC1 16 specimens, coefficient of variation 4.75 % (SAR Tables 5-2 and 5-8) | 0.334 | 0.31985 | −4.24 % | Within 10 % |
| Soft, RTD modulus [Msi], Poisson's ratio, νxy compression Specimens: UNT2 18 specimens, coefficient of variation 5.27 %; UNC2 16 specimens, coefficient of variation 6.10 % (SAR Tables 5-4 and 5-10) | 0.587 | 0.56475 | −3.79 % | Within 10 % |
| Cross-ply compression, RTD modulus [Msi], Poisson's ratio, νxy compression Specimens: UNC0 9 specimens, coefficient of variation 2.62 % (SAR Table 4-16) | 0.035 | 0.036295 | +3.70 % | Within 10 % |
| Soft, CTD modulus [Msi], Poisson's ratio, Ex tension Specimens: UNT2 17 specimens, coefficient of variation 2.03 % (SAR Table 5-4) | 5.52 | 5.7198 | +3.62 % | Within 10 % |
| Hard, RTD modulus [Msi], Poisson's ratio, νxy compression Specimens: UNT3 22 specimens, coefficient of variation 6.04 %; UNC3 17 specimens, coefficient of variation 4.35 % (SAR Tables 5-6 and 5-12) | 0.423 | 0.43587 | +3.04 % | Within 10 % |
| Hard, CTD modulus [Msi], Poisson's ratio, Ex tension Specimens: UNT3 19 specimens, coefficient of variation 1.98 % (SAR Table 5-6) | 13.11 | 13.347 | +1.81 % | Within 10 % |
| Cross-ply tension, RTD modulus [Msi], Poisson's ratio, Ex tension Specimens: UNT0 18 specimens, coefficient of variation 1.76 % (SAR Table 4-14) | 11.99 | 12.2 | +1.75 % | Within 10 % |
| Cross-ply tension, CTD modulus [Msi], Poisson's ratio, Ex tension Specimens: UNT0 19 specimens, coefficient of variation 1.24 % (SAR Table 4-14) | 11.92 | 12.059 | +1.17 % | Within 10 % |
How to reproduce it
Source
NCAMP, "Hexcel 8552 IM7 Unidirectional Prepreg 190 gsm & 35%RC Qualification Statistical Analysis Report", NCP-RP-2009-028 Rev B, April 16, 2019. Stacking sequences from the Material Property Data Report CAM-RP-2009-015 Rev B, April 16, 2019.
SAR Tables 3-3 and 3-4, Sections 4 and 5; stacking sequences MPDR Table 1-2
What was taken from it
Mean measured laminate moduli in tension and compression and the compression Poisson's ratios, normalized to 0.0072 in per ply, in three environments. CLT is built from the lamina values of the same report and environment.
Quantity compared: modulus [Msi], Poisson's ratio
Inputs
- Ply at RTD, SAR Table 3-3: tension E1 22.99 Msi, E2 1.30 Msi, G12 0.68 Msi, ν12 0.316; compression E1 20.04 Msi, E2 1.41 Msi, ν12 0.356
- CTD and ETW use the lamina values of their own environment from the same table
- Tension cases use the tension lamina values, compression cases the compression values
- Lamina and laminate moduli are both chord values between 1000 and 3000 µε
The inputs of each configuration are listed in the table below.
Allowed difference
10 %; ±10 %, known gap
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Cross-ply compression, ETW, νxy compression | cross-ply | 0.017 | 0.032343 | +90.3 % |
| Hard, ETW, νxy compression | none | 0.416 | 0.47917 | +15.2 % |
| Quasi-isotropic, ETW, Ex tension | quasi-isotropic | 7.99 | 8.5178 | +6.61 % |
| Soft, ETW, Ex tension | none | 4.47 | 4.7625 | +6.54 % |
| Cross-ply compression, CTD, νxy compression | cross-ply | 0.041 | 0.03874 | −5.51 % |
| Soft, ETW, νxy compression | none | 0.665 | 0.62906 | −5.40 % |
| Cross-ply tension, ETW, Ex tension | cross-ply | 11.94 | 12.462 | +4.37 % |
| Quasi-isotropic, CTD, Ex tension | quasi-isotropic | 8.35 | 8.7144 | +4.36 % |
| Quasi-isotropic, RTD, νxy compression | quasi-isotropic | 0.334 | 0.31985 | −4.24 % |
| Quasi-isotropic, ETW, Ex compression | quasi-isotropic | 7.13 | 7.418 | +4.04 % |
| Soft, RTD, νxy compression | none | 0.587 | 0.56475 | −3.79 % |
| Soft, RTD, Ex tension | none | 5.22 | 5.4171 | +3.78 % |
| Cross-ply compression, RTD, νxy compression | cross-ply | 0.035 | 0.036295 | +3.70 % |
| Soft, CTD, Ex tension | none | 5.52 | 5.7198 | +3.62 % |
| Hard, ETW, Ex tension | none | 13.14 | 13.573 | +3.29 % |
| Quasi-isotropic, ETW, νxy compression | quasi-isotropic | 0.356 | 0.34488 | −3.12 % |
| Quasi-isotropic, RTD, Ex tension | quasi-isotropic | 8.39 | 8.652 | +3.12 % |
| Hard, RTD, νxy compression | none | 0.423 | 0.43587 | +3.04 % |
| Cross-ply compression, CTD, Ex compression | cross-ply | 7.75 | 7.9691 | +2.83 % |
| Cross-ply compression, RTD, Ex compression | cross-ply | 7.47 | 7.6702 | +2.68 % |
| Soft, ETW, Ex compression | none | 4.1 | 4.2002 | +2.44 % |
| Quasi-isotropic, RTD, Ex compression | quasi-isotropic | 7.86 | 7.7047 | −1.98 % |
| Hard, RTD, Ex tension | none | 13.15 | 13.403 | +1.92 % |
| Hard, CTD, Ex tension | none | 13.11 | 13.347 | +1.81 % |
| Cross-ply tension, RTD, Ex tension | cross-ply | 11.99 | 12.2 | +1.75 % |
| Cross-ply compression, ETW, Ex compression | cross-ply | 7.74 | 7.6269 | −1.46 % |
| Hard, ETW, Ex compression | none | 11.77 | 11.623 | −1.25 % |
| Cross-ply tension, CTD, Ex tension | cross-ply | 11.92 | 12.059 | +1.17 % |
| Hard, RTD, Ex compression | none | 11.9 | 11.789 | −0.94 % |
| Soft, RTD, Ex compression | none | 4.9 | 4.9305 | +0.62 % |
Bowles, D. E., Post, D., Herakovich, C. T. & Tenney, D. R., "Thermal Expansion of Composites Using Moire Interferometry", VPI-E-80-19, NASA-Virginia Tech Composites Program Interim Report 20, August 1980.
Measured
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| T300/5208 [0/90/±45]s α<sub>x</sub> (10⁻⁶/°C), αx, strain gageWhy: The strain gages read 0.45 to 0.52 x 10⁻⁶/°C higher than moiré on the same laminate. The ply α1 and α2 entered here are the moiré values, so the prediction follows the moiré reading. | 2.5 | 1.838 | −26.5 % | Known gap |
| T300/5208 [0/±45/90]s α<sub>x</sub> (10⁻⁶/°C), αx, strain gageWhy: The strain gages read 0.45 to 0.52 x 10⁻⁶/°C higher than moiré on the same laminate. The ply α1 and α2 entered here are the moiré values, so the prediction follows the moiré reading. | 2.41 | 1.838 | −23.7 % | Known gap |
How to reproduce it
Source
Bowles, D. E., Post, D., Herakovich, C. T. & Tenney, D. R., "Thermal Expansion of Composites Using Moire Interferometry", VPI-E-80-19, NASA-Virginia Tech Composites Program Interim Report 20, August 1980.
Table 3 (CTE at 297 K), Table 4 (ply stiffness)
What was taken from it
CTE of two quasi-isotropic laminates at 297 K, measured by moiré interferometry and by strain gages on the same specimens. The ply α1 and α2 are the report's own [0] and [90] measurements.
Quantity compared: α<sub>x</sub> (10⁻⁶/°C)
Inputs
- Ply E1 130.3 GPa, E2 9.72 GPa, G12 5.39 GPa, ν12 0.308 (Table 4, dry)
- Ply α1 -0.107 and α2 22.23 x 10⁻⁶/°C, the moiré values at 297 K in Table 3
- Both layups are quasi-isotropic, so αy equals αx and only αx is compared
The inputs of each configuration are listed in the table below.
Allowed difference
20 %, or 0.5 x 10⁻⁶/°C, whichever is larger
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| T300/5208 [0/90/±45]s, αx, strain gage | quasi-isotropic | 2.5 | 1.838 | −26.5 % |
| T300/5208 [0/±45/90]s, αx, strain gage | quasi-isotropic | 2.41 | 1.838 | −23.7 % |
| T300/5208 [0/90/±45]s, αx, moiré | quasi-isotropic | 2.05 | 1.838 | −8.48 % |
| T300/5208 [0/±45/90]s, αx, moiré | quasi-isotropic | 1.89 | 1.838 | −2.08 % |
NCAMP, "Victrex LMPAEK AS4 Unidirectional Tape Qualification Statistical Analysis Report", NCP-RP-2021-015 Rev N/C, January 13, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2021-025 Rev N/C, January 13, 2026.
Measured [Msi]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Soft, ETW modulus [Msi], Ex tensionWhy: Hot and wet, and 80 % of the plies sit at ±45°, so the modulus leans on G12 and E2, the lamina values moisture softens most. The report prints no transverse tension modulus, so the compression value stands in for it. | 3.516 | 4.1591 | +18.3 % | Known gap |
| Quasi-isotropic, ETW modulus [Msi], Ex tensionWhy: Hot and wet, the softened matrix carries more of the load. The report prints no transverse tension modulus, so the compression value stands in for it. | 6.486 | 7.1538 | +10.3 % | Known gap |
| Hard, ETW modulus [Msi], Ex tension | 10.35 | 11.222 | +8.43 % | Within 10 % |
| Quasi-isotropic, CTA modulus [Msi], Ex tension | 7.067 | 7.3862 | +4.52 % | Within 10 % |
| Quasi-isotropic, ETA modulus [Msi], Ex compression | 6.34 | 6.6209 | +4.43 % | Within 10 % |
| Soft, CTA modulus [Msi], Ex tension | 4.602 | 4.799 | +4.28 % | Within 10 % |
| Soft, RTA modulus [Msi], Ex tension | 4.553 | 4.7272 | +3.83 % | Within 10 % |
| Hard, RTA modulus [Msi], Ex tension | 10.98 | 11.26 | +2.55 % | Within 10 % |
| Hard, CTA modulus [Msi], Ex tension | 10.96 | 11.225 | +2.42 % | Within 10 % |
| Quasi-isotropic, RTA modulus [Msi], Ex tension | 7.259 | 7.3667 | +1.48 % | Within 10 % |
How to reproduce it
Source
NCAMP, "Victrex LMPAEK AS4 Unidirectional Tape Qualification Statistical Analysis Report", NCP-RP-2021-015 Rev N/C, January 13, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2021-025 Rev N/C, January 13, 2026.
SAR Tables 3-3 and 3-4; stacking sequences MPDR p. 18
What was taken from it
Mean measured laminate moduli in tension and compression, normalized to 0.0054 in per ply, in four environments. The report prints no laminate Poisson's ratio. CLT is built from the lamina values of the same report and environment.
Quantity compared: modulus [Msi]
Inputs
- Ply at RTA, SAR Table 3-3: tension E1 19.10 Msi, ν12 0.2836; compression E1 16.91 Msi, ν12 0.3363; E2 1.406 Msi, G12 0.6562 Msi
- CTA, ETA and ETW use the lamina values of their own environment from the same table
- The report prints no transverse tension modulus, so E2 from the transverse compression test serves the tension cases too
- Lamina and laminate moduli are both chord values between 1000 and 3000 µε
The inputs of each configuration are listed in the table below.
Allowed difference
10 %; ±10 %, known gap
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Soft, ETW, Ex tension | none | 3.516 | 4.1591 | +18.3 % |
| Quasi-isotropic, ETW, Ex tension | quasi-isotropic | 6.486 | 7.1538 | +10.3 % |
| Hard, ETW, Ex tension | none | 10.35 | 11.222 | +8.43 % |
| Quasi-isotropic, ETW, Ex compression | quasi-isotropic | 6.024 | 6.3747 | +5.82 % |
| Hard, ETW, Ex compression | none | 9.47 | 9.9278 | +4.83 % |
| Soft, ETW, Ex compression | none | 3.598 | 3.7631 | +4.59 % |
| Quasi-isotropic, CTA, Ex tension | quasi-isotropic | 7.067 | 7.3862 | +4.52 % |
| Quasi-isotropic, ETA, Ex compression | quasi-isotropic | 6.34 | 6.6209 | +4.43 % |
| Soft, CTA, Ex tension | none | 4.602 | 4.799 | +4.28 % |
| Soft, RTA, Ex tension | none | 4.553 | 4.7272 | +3.83 % |
| Quasi-isotropic, ETA, Ex tension | quasi-isotropic | 6.654 | 6.8699 | +3.24 % |
| Hard, RTA, Ex tension | none | 10.98 | 11.26 | +2.55 % |
| Hard, CTA, Ex tension | none | 10.96 | 11.225 | +2.42 % |
| Quasi-isotropic, RTA, Ex tension | quasi-isotropic | 7.259 | 7.3667 | +1.48 % |
| Soft, RTA, Ex compression | none | 4.308 | 4.352 | +1.02 % |
| Hard, RTA, Ex compression | none | 9.98 | 10.046 | +0.66 % |
| Quasi-isotropic, RTA, Ex compression | quasi-isotropic | 6.599 | 6.6386 | +0.60 % |
Clay, S. B. & Knoth, P. M., "Experimental Results of Quasi-Static Testing for Calibration and Validation of Composite Progressive Damage Analysis Methods", J Compos Mater 51 (2017) 1333-1353.
Measured [GPa]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| [0/45/90/-45]2S modulus [GPa], Ex compression Specimens: tension 56.9 to 60.9 GPa, compression 45.5 to 50.4 GPa (90 % bounds) (Table 3 and p. 17) | 48 | 52.675 | +9.74 % | Within 10 % |
| [30/60/90/-60/-30]2S modulus [GPa], Ex tension Specimens: tension 37.3 to 38.9 GPa, compression 28.3 to 38.7 GPa (90 % bounds) (Table 3 and p. 17) | 38.1 | 41.32 | +8.45 % | Within 10 % |
| [60/0/-60]3S modulus [GPa], Ex compression Specimens: tension 57.8 to 61.3 GPa, compression 47.3 to 50.5 GPa (90 % bounds) (Table 3 and p. 17) | 48.9 | 52.675 | +7.72 % | Within 10 % |
How to reproduce it
Source
Clay, S. B. & Knoth, P. M., "Experimental Results of Quasi-Static Testing for Calibration and Validation of Composite Progressive Damage Analysis Methods", J Compos Mater 51 (2017) 1333-1353.
Table 3 (laminate moduli), Table 2 (ply properties), p. 17 (bounds)
What was taken from it
Mean measured laminate moduli in tension and compression for three layups. CLT is built from the ply properties measured in the same program.
Quantity compared: modulus [GPa]
Inputs
- IM7/977-3 ply, Table 2: tension E1 164 GPa, E2 8.98 GPa; compression E1 137 GPa, E2 8.69 GPa; G12 5.01 GPa; ν12 0.320, measured in tension and used for both
The inputs of each configuration are listed in the table below.
Allowed difference
10 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| [0/45/90/-45]2S, Ex compression | quasi-isotropic | 48 | 52.675 | +9.74 % |
| [30/60/90/-60/-30]2S, Ex tension | none | 38.1 | 41.32 | +8.45 % |
| [60/0/-60]3S, Ex compression | quasi-isotropic | 48.9 | 52.675 | +7.72 % |
| [30/60/90/-60/-30]2S, Ex compression | none | 33.5 | 35.81 | +6.89 % |
| [0/45/90/-45]2S, Ex tension | quasi-isotropic | 58.9 | 61.767 | +4.87 % |
| [60/0/-60]3S, Ex tension | quasi-isotropic | 59.5 | 61.767 | +3.81 % |
Ueki, Y., Lilholt, H. & Madsen, B., "Experimental Evaluation of Stiffness Predictions of Multiaxial Flax Fibre Composites by Classical Laminate Theory", PLoS One 15(6) (2020) e0234701.
Measured [GPa]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Fabric I, layup B, 45° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 12.2 | 11.083 | −9.16 % | Within 10 % |
| Fabric I, layup A, 45° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 12.5 | 11.457 | −8.34 % | Within 10 % |
| Fabric II, layup A, 45° modulus [GPa], Ex tension Specimens: 3 tested, ±0.4 GPa (Table 4) | 12.2 | 11.83 | −3.03 % | Within 10 % |
| Fabric I, layup A, 0° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 5.7 | 5.5414 | −2.78 % | Within 10 % |
| Fabric I, layup A, 90° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 6.1 | 5.9499 | −2.46 % | Within 10 % |
| Fabric II, layup B, 90° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 6.1 | 6.2497 | +2.45 % | Within 10 % |
| Fabric I, layup B, 90° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 6.9 | 7.0572 | +2.28 % | Within 10 % |
| Fabric II, layup B, 0° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 5.1 | 5.206 | +2.08 % | Within 10 % |
| Fabric I, layup B, 0° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 4.6 | 4.5136 | −1.88 % | Within 10 % |
| Fabric II, layup A, 90° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 5.3 | 5.3743 | +1.40 % | Within 10 % |
| Fabric II, layup A, 0° modulus [GPa], Ex tension Specimens: 3 tested, ±0.1 GPa (Table 4) | 5.7 | 5.6256 | −1.31 % | Within 10 % |
| Fabric II, layup B, 45° modulus [GPa], Ex tension Specimens: 3 tested, ±0.5 GPa (Table 4) | 11.6 | 11.452 | −1.28 % | Within 10 % |
How to reproduce it
Source
Ueki, Y., Lilholt, H. & Madsen, B., "Experimental Evaluation of Stiffness Predictions of Multiaxial Flax Fibre Composites by Classical Laminate Theory", PLoS One 15(6) (2020) e0234701.
Table 4 (measured moduli), Table 3 (measured ply angles), p. 13 (ply properties)
What was taken from it
Mean measured tensile moduli of two non-crimp flax fabrics in two layups, each tested at 0°, 45° and 90°. CLT uses the ply angles measured on the specimens and the full ABD inverse, since the measured stacks are unsymmetric.
Quantity compared: modulus [GPa]
Inputs
- Flax/epoxy ply, p. 13: E1 19.8 GPa, E2 3.7 GPa, G12 1.7 GPa, ν12 0.30. E1 is the measured unidirectional modulus scaled to 31 % fiber volume; E2, G12 and ν12 are the paper's micromechanics estimates
- 8 equal plies, ply 1 on top
The inputs of each configuration are listed in the table below.
Allowed difference
10 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Fabric I, layup B, 45°, Ex tension | unsymmetric | 12.2 | 11.083 | −9.16 % |
| Fabric I, layup A, 45°, Ex tension | unsymmetric | 12.5 | 11.457 | −8.34 % |
| Fabric II, layup A, 45°, Ex tension | unsymmetric | 12.2 | 11.83 | −3.03 % |
| Fabric I, layup A, 0°, Ex tension | unsymmetric | 5.7 | 5.5414 | −2.78 % |
| Fabric I, layup A, 90°, Ex tension | unsymmetric | 6.1 | 5.9499 | −2.46 % |
| Fabric II, layup B, 90°, Ex tension | unsymmetric | 6.1 | 6.2497 | +2.45 % |
| Fabric I, layup B, 90°, Ex tension | unsymmetric | 6.9 | 7.0572 | +2.28 % |
| Fabric II, layup B, 0°, Ex tension | unsymmetric | 5.1 | 5.206 | +2.08 % |
| Fabric I, layup B, 0°, Ex tension | unsymmetric | 4.6 | 4.5136 | −1.88 % |
| Fabric II, layup A, 90°, Ex tension | unsymmetric | 5.3 | 5.3743 | +1.40 % |
| Fabric II, layup A, 0°, Ex tension | unsymmetric | 5.7 | 5.6256 | −1.31 % |
| Fabric II, layup B, 45°, Ex tension | unsymmetric | 11.6 | 11.452 | −1.28 % |
NCAMP, "Toray Cetex TC1225 (LM PAEK) T700GC 145 gsm 34% RC Unsized Fiber Unidirectional Slit Tape Material Allowables Statistical Analysis Report", NCP-RP-2025-008 Rev A, February 24, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2025-016 Rev A, February 24, 2026.
Measured [Msi]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Soft, ETA1 modulus [Msi], Ex compression | 4.191 | 3.8098 | −9.10 % | Within 10 % |
| Quasi-isotropic, ETW modulus [Msi], Ex tension | 6.511 | 6.924 | +6.34 % | Within 10 % |
| Quasi-isotropic, ETA1 modulus [Msi], Ex tension | 6.855 | 7.247 | +5.72 % | Within 10 % |
| Quasi-isotropic, RTA modulus [Msi], Ex tension | 7.106 | 7.3994 | +4.13 % | Within 10 % |
| Soft, CTA modulus [Msi], Ex tension | 4.68 | 4.8554 | +3.75 % | Within 10 % |
| Soft, RTA modulus [Msi], Ex tension | 4.516 | 4.6793 | +3.62 % | Within 10 % |
| Quasi-isotropic, CTA modulus [Msi], Ex tension | 7.256 | 7.5168 | +3.59 % | Within 10 % |
| Hard, ETA1 modulus [Msi], Ex tension | 11.06 | 11.383 | +2.92 % | Within 10 % |
| Hard, CTA modulus [Msi], Ex tension | 11.21 | 11.477 | +2.38 % | Within 10 % |
| Cross-ply UNC0, CTA modulus [Msi], Ex compression | 9.569 | 9.7681 | +2.08 % | Within 10 % |
| Hard, RTA modulus [Msi], Ex tension | 11.15 | 11.36 | +1.88 % | Within 10 % |
| Cross-ply UNC0, ETW modulus [Msi], Ex compression | 9.356 | 9.1971 | −1.70 % | Within 10 % |
| Cross-ply UNC0, RTA modulus [Msi], Ex compression | 9.43 | 9.5862 | +1.66 % | Within 10 % |
| Cross-ply UNC0, ETA1 modulus [Msi], Ex compression | 9.743 | 9.7106 | −0.33 % | Within 10 % |
How to reproduce it
Source
NCAMP, "Toray Cetex TC1225 (LM PAEK) T700GC 145 gsm 34% RC Unsized Fiber Unidirectional Slit Tape Material Allowables Statistical Analysis Report", NCP-RP-2025-008 Rev A, February 24, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2025-016 Rev A, February 24, 2026.
SAR Tables 3-3 and 3-4; stacking sequences MPDR Tables 1-2 and 1-3, pp. 18 and 20
What was taken from it
Mean measured laminate moduli in tension and compression, normalized to 0.0054 in per ply, in four environments, and the compression modulus of a [90/0]4S cross-ply. The report prints no laminate Poisson's ratio. CLT is built from the lamina values of the same report and environment.
Quantity compared: modulus [Msi]
Inputs
- Ply at RTA, SAR Table 3-3: tension E1 19.38 Msi, E2 1.316 Msi, ν12 0.3499; compression E1 17.66 Msi, E2 1.386 Msi, ν12 0.3389; G12 0.6157 Msi
- CTA, ETA1 and ETW use the lamina values of their own environment from the same table
- ETW has quasi-isotropic and cross-ply values only
- ETA2 (400 °F) is left out: it is above the dry Tg of 291 °F
The inputs of each configuration are listed in the table below.
Allowed difference
10 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Soft, ETA1, Ex compression | none | 4.191 | 3.8098 | −9.10 % |
| Quasi-isotropic, ETW, Ex tension | none | 6.511 | 6.924 | +6.34 % |
| Quasi-isotropic, ETA1, Ex tension | none | 6.855 | 7.247 | +5.72 % |
| Soft, ETA1, Ex tension | none | 3.92 | 4.1098 | +4.84 % |
| Quasi-isotropic, RTA, Ex tension | none | 7.106 | 7.3994 | +4.13 % |
| Soft, CTA, Ex tension | none | 4.68 | 4.8554 | +3.75 % |
| Soft, RTA, Ex tension | none | 4.516 | 4.6793 | +3.62 % |
| Quasi-isotropic, CTA, Ex tension | none | 7.256 | 7.5168 | +3.59 % |
| Quasi-isotropic, ETW, Ex compression | none | 6.488 | 6.2577 | −3.55 % |
| Hard, ETA1, Ex tension | none | 11.06 | 11.383 | +2.92 % |
| Hard, CTA, Ex tension | none | 11.21 | 11.477 | +2.38 % |
| Cross-ply UNC0, CTA, Ex compression | none | 9.569 | 9.7681 | +2.08 % |
| Quasi-isotropic, RTA, Ex compression | none | 6.72 | 6.8472 | +1.89 % |
| Hard, RTA, Ex tension | none | 11.15 | 11.36 | +1.88 % |
| Cross-ply UNC0, ETW, Ex compression | none | 9.356 | 9.1971 | −1.70 % |
| Cross-ply UNC0, RTA, Ex compression | none | 9.43 | 9.5862 | +1.66 % |
| Hard, ETA1, Ex compression | none | 10.51 | 10.37 | −1.33 % |
| Soft, RTA, Ex compression | none | 4.449 | 4.3979 | −1.15 % |
| Quasi-isotropic, ETA1, Ex compression | none | 6.736 | 6.6589 | −1.14 % |
| Hard, RTA, Ex compression | none | 10.38 | 10.423 | +0.42 % |
| Cross-ply UNC0, ETA1, Ex compression | none | 9.743 | 9.7106 | −0.33 % |
Lovejoy, A. E., Scotti, S. J., Miller, S. G., Heimann, P. & Miller, S. S., "Characterization of IM7/8552 Thin-ply and Hybrid Thin-ply Composites", AIAA SciTech 2019, NTRS 20200002400.
Measured
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| 70 gsm, hybrid, thin ±45 plies modulus [Msi], Poisson's ratio, νxy tension Specimens: averages only, no scatter printed (Table 2) | 0.396 | 0.37087 | −6.35 % | Within 10 % |
| 30 gsm, hybrid, thin ±45 plies modulus [Msi], Poisson's ratio, νxy tension Specimens: averages only, no scatter printed (Table 2) | 0.263 | 0.24946 | −5.15 % | Within 10 % |
| 30 gsm, quasi-isotropic modulus [Msi], Poisson's ratio, νxy tension Specimens: averages only, no scatter printed (Table 2) | 0.306 | 0.31996 | +4.56 % | Within 10 % |
| 70 gsm, quasi-isotropic modulus [Msi], Poisson's ratio, νxy compression Specimens: averages only, no scatter printed (Table 2) | 0.306 | 0.31753 | +3.77 % | Within 10 % |
| 30 gsm, cross-ply modulus [Msi], Poisson's ratio, Ex compression Specimens: averages only, no scatter printed (Table 2) | 11 | 10.622 | −3.44 % | Within 10 % |
| 70 gsm, cross-ply modulus [Msi], Poisson's ratio, νxy compression Specimens: averages only, no scatter printed (Table 2) | 0.048 | 0.049167 | +2.43 % | Within 10 % |
How to reproduce it
Source
Lovejoy, A. E., Scotti, S. J., Miller, S. G., Heimann, P. & Miller, S. S., "Characterization of IM7/8552 Thin-ply and Hybrid Thin-ply Composites", AIAA SciTech 2019, NTRS 20200002400.
Tables 3 and 4 (laminate and lamina moduli), Table 7 (G12), Table 1 (stacking sequences)
What was taken from it
Mean measured laminate moduli and Poisson's ratios in tension and compression for 30 gsm and 70 gsm plies, and for hybrids with thin ±45° plies between standard 190 gsm plies. CLT is built from the lamina values the paper measured for each grade.
Quantity compared: modulus [Msi], Poisson's ratio
Inputs
- 30 gsm ply, Tables 3, 4 and 7: tension E1 21.29 Msi, E2 1.49 Msi, ν12 0.349; compression E1 19.70 Msi, E2 1.39 Msi, ν12 0.368; G12 0.707 Msi; cured ply 0.0012 in
- 70 gsm ply, same tables: tension E1 21.22 Msi, E2 1.42 Msi, ν12 0.347; compression E1 19.50 Msi, E2 1.40 Msi, ν12 0.367; G12 0.718 Msi; cured ply 0.0028 in
- Standard 190 gsm ply in the hybrids, the NCAMP rows of the same tables: tension E1 22.99 Msi, E2 1.3 Msi, ν12 0.316; compression E1 20.04 Msi, E2 1.41 Msi, ν12 0.356; G12 0.680 Msi; ply 0.0072 in
The inputs of each configuration are listed in the table below.
Allowed difference
10 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| 70 gsm, hybrid, thin ±45 plies, νxy tension | none | 0.396 | 0.37087 | −6.35 % |
| 30 gsm, hybrid, thin ±45 plies, νxy tension | none | 0.263 | 0.24946 | −5.15 % |
| 30 gsm, quasi-isotropic, νxy tension | quasi-isotropic | 0.306 | 0.31996 | +4.56 % |
| 70 gsm, hybrid, thin ±45 plies, Ex compression | none | 13.95 | 13.359 | −4.24 % |
| 70 gsm, quasi-isotropic, νxy compression | quasi-isotropic | 0.306 | 0.31753 | +3.77 % |
| 30 gsm, cross-ply, Ex compression | cross-ply | 11 | 10.622 | −3.44 % |
| 30 gsm, quasi-isotropic, νxy compression | quasi-isotropic | 0.329 | 0.31833 | −3.24 % |
| 70 gsm, hybrid, thin ±45 plies, νxy compression | none | 0.397 | 0.38441 | −3.17 % |
| 70 gsm, quasi-isotropic, Ex compression | quasi-isotropic | 7.79 | 7.5555 | −3.01 % |
| 30 gsm, hybrid, thin ±45 plies, Ex compression | none | 15.86 | 15.41 | −2.84 % |
| 30 gsm, hybrid, thin ±45 plies, Ex tension | none | 17.13 | 17.58 | +2.63 % |
| 70 gsm, cross-ply, νxy compression | cross-ply | 0.048 | 0.049167 | +2.43 % |
| 70 gsm, quasi-isotropic, νxy tension | quasi-isotropic | 0.31 | 0.31702 | +2.26 % |
| 30 gsm, quasi-isotropic, Ex compression | quasi-isotropic | 7.76 | 7.6096 | −1.94 % |
| 70 gsm, hybrid, thin ±45 plies, Ex tension | none | 14.98 | 15.199 | +1.46 % |
| 70 gsm, cross-ply, Ex compression | cross-ply | 10.64 | 10.527 | −1.07 % |
| 30 gsm, cross-ply, νxy compression | cross-ply | 0.048 | 0.048508 | +1.06 % |
| 30 gsm, hybrid, thin ±45 plies, νxy compression | none | 0.273 | 0.27045 | −0.93 % |
| 30 gsm, quasi-isotropic, Ex tension | quasi-isotropic | 8.22 | 8.1689 | −0.62 % |
| 70 gsm, quasi-isotropic, Ex tension | quasi-isotropic | 8.12 | 8.1334 | +0.16 % |
Tompkins, S. S., "Thermal Expansion of Selected Graphite Reinforced Polyimide-, Epoxy-, and Glass-Matrix Composites", NASA TM-87572, July 1985.
Measured
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| P75S/930 cross-ply α<sub>x</sub> (10⁻⁶/°C), αx | -0.533 | -0.38485 | +5.93 % | Within 10 % |
| C6000/PMR-15 quasi-isotropic α<sub>x</sub> (10⁻⁶/°C), αx | 1.529 | 1.6434 | +4.58 % | Within 10 % |
| P75S/CE339 cross-ply α<sub>x</sub> (10⁻⁶/°C), αx | 0.76 | 0.64952 | −4.42 % | Within 10 % |
| C6000/PMR-15 cross-ply α<sub>x</sub> (10⁻⁶/°C), αx | 1.635 | 1.6434 | +0.34 % | Within 10 % |
| P75S/934 cross-ply α<sub>x</sub> (10⁻⁶/°C), αx | -0.181 | -0.18483 | −0.15 % | Within 10 % |
How to reproduce it
Source
Tompkins, S. S., "Thermal Expansion of Selected Graphite Reinforced Polyimide-, Epoxy-, and Glass-Matrix Composites", NASA TM-87572, July 1985.
Table II (laminates), Table I (ply properties)
What was taken from it
Laminate CTE at 24 °C, measured with a laser interferometric dilatometer on dried specimens, two or three tests per laminate. CLT is built from the ply properties the report lists for its own predictions.
Quantity compared: α<sub>x</sub> (10⁻⁶/°C)
Inputs
- Ply E1, E2, G12, ν12, α1 and α2 at 24 °C exactly as Table I prints them
- Table I takes the ply properties from the literature, not from the measured panels
- Each laminate was measured along one axis. In these layups αy equals αx, so only αx is compared
- The carbon/glass laminate is left out because Table I lists no ply properties for it
The inputs of each configuration are listed in the table below.
Allowed difference
20 %, or 0.5 x 10⁻⁶/°C, whichever is larger
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| P75S/930 cross-ply, αx | cross-ply | -0.533 | -0.38485 | +5.93 % |
| C6000/PMR-15 quasi-isotropic, αx | quasi-isotropic | 1.529 | 1.6434 | +4.58 % |
| P75S/CE339 cross-ply, αx | cross-ply | 0.76 | 0.64952 | −4.42 % |
| C6000/PMR-15 cross-ply, αx | cross-ply | 1.635 | 1.6434 | +0.34 % |
| P75S/934 cross-ply, αx | cross-ply | -0.181 | -0.18483 | −0.15 % |
NCAMP, "Toray Advanced Composites TC380 T1100GC 24K 120gsm Unitape with 35% RC Material Allowables Statistical Analysis Report", NCP-RP-2025-010 Rev A, September 18, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2025-021 Rev A, September 17, 2026.
Measured [Msi]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Soft, ETW2 modulus [Msi], Ex tension | 4.48 | 4.71 | +5.13 % | Within 10 % |
| Cross-ply UNC0, CTD modulus [Msi], Ex compression | 7.818 | 8.1523 | +4.28 % | Within 10 % |
| Soft, ETW1 modulus [Msi], Ex tension | 4.699 | 4.8805 | +3.86 % | Within 10 % |
| Soft, RTD modulus [Msi], Ex tension | 4.933 | 5.1228 | +3.85 % | Within 10 % |
| Quasi-isotropic, ETW2 modulus [Msi], Ex tension | 8.128 | 8.4164 | +3.55 % | Within 10 % |
| Quasi-isotropic, ETW1 modulus [Msi], Ex compression | 7.545 | 7.8101 | +3.51 % | Within 10 % |
| Soft, CTD modulus [Msi], Ex tension | 5.349 | 5.4816 | +2.48 % | Within 10 % |
| Hard, RTD modulus [Msi], Ex compression | 12.41 | 12.104 | −2.46 % | Within 10 % |
| Quasi-isotropic, CTD modulus [Msi], Ex tension | 8.6 | 8.8117 | +2.46 % | Within 10 % |
| Hard, ETW1 modulus [Msi], Ex compression | 11.98 | 12.27 | +2.42 % | Within 10 % |
| Quasi-isotropic, RTD modulus [Msi], Ex tension | 8.254 | 8.4374 | +2.22 % | Within 10 % |
| Cross-ply UNC0, ETW1 modulus [Msi], Ex compression | 7.76 | 7.8786 | +1.53 % | Within 10 % |
| Soft, ETD1 modulus [Msi], Ex compression | 4.683 | 4.7401 | +1.22 % | Within 10 % |
| Hard, ETW2 modulus [Msi], Ex tension | 13.59 | 13.439 | −1.11 % | Within 10 % |
| Cross-ply UNC0, ETD1 modulus [Msi], Ex compression | 7.858 | 7.9269 | +0.88 % | Within 10 % |
| Cross-ply UNC0, RTD modulus [Msi], Ex compression | 7.729 | 7.7942 | +0.84 % | Within 10 % |
| Hard, ETD1 modulus [Msi], Ex compression | 12.46 | 12.355 | −0.84 % | Within 10 % |
| Hard, CTD modulus [Msi], Ex compression | 12.57 | 12.657 | +0.69 % | Within 10 % |
| Quasi-isotropic, ETD1 modulus [Msi], Ex compression | 7.878 | 7.9093 | +0.40 % | Within 10 % |
| Cross-ply UNC0, ETW2 modulus [Msi], Ex compression | 7.688 | 7.699 | +0.14 % | Within 10 % |
How to reproduce it
Source
NCAMP, "Toray Advanced Composites TC380 T1100GC 24K 120gsm Unitape with 35% RC Material Allowables Statistical Analysis Report", NCP-RP-2025-010 Rev A, September 18, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2025-021 Rev A, September 17, 2026.
SAR Tables 3-3 and 3-4; stacking sequences MPDR Table 1-3, p. 23, and p. 21
What was taken from it
Mean measured laminate moduli in tension and compression, normalized to 0.0048 in per ply, in five environments, and the compression modulus of a [90/0/90]7 cross-ply. CLT is built from the lamina values of the same report and environment.
Quantity compared: modulus [Msi]
Inputs
- Ply at RTD, SAR Table 3-3: tension E1 22.84 Msi, E2 1.108 Msi, ν12 0.3132; compression E1 20.85 Msi, E2 1.198 Msi, ν12 0.3621; G12 0.5582 Msi
- E1 is normalized to the cured ply thickness; E2, G12 and ν12 are as measured
- CTD, ETD1, ETW1 and ETW2 use the lamina values of their own environment from the same table
- ETD1 has laminate values in compression only
The inputs of each configuration are listed in the table below.
Allowed difference
10 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Soft, ETW2, Ex tension | none | 4.48 | 4.71 | +5.13 % |
| Cross-ply UNC0, CTD, Ex compression | none | 7.818 | 8.1523 | +4.28 % |
| Soft, ETW1, Ex tension | none | 4.699 | 4.8805 | +3.86 % |
| Soft, RTD, Ex tension | none | 4.933 | 5.1228 | +3.85 % |
| Quasi-isotropic, ETW2, Ex tension | none | 8.128 | 8.4164 | +3.55 % |
| Quasi-isotropic, ETW1, Ex compression | none | 7.545 | 7.8101 | +3.51 % |
| Soft, ETW1, Ex compression | none | 4.411 | 4.5491 | +3.13 % |
| Soft, CTD, Ex tension | none | 5.349 | 5.4816 | +2.48 % |
| Hard, RTD, Ex compression | none | 12.41 | 12.104 | −2.46 % |
| Quasi-isotropic, CTD, Ex tension | none | 8.6 | 8.8117 | +2.46 % |
| Hard, ETW1, Ex compression | none | 11.98 | 12.27 | +2.42 % |
| Quasi-isotropic, ETW2, Ex compression | none | 7.433 | 7.6114 | +2.40 % |
| Quasi-isotropic, RTD, Ex tension | none | 8.254 | 8.4374 | +2.22 % |
| Quasi-isotropic, CTD, Ex compression | none | 8.047 | 8.2079 | +2.00 % |
| Quasi-isotropic, ETW1, Ex tension | none | 8.299 | 8.4514 | +1.84 % |
| Cross-ply UNC0, ETW1, Ex compression | none | 7.76 | 7.8786 | +1.53 % |
| Soft, RTD, Ex compression | none | 4.865 | 4.7967 | −1.40 % |
| Soft, ETD1, Ex compression | none | 4.683 | 4.7401 | +1.22 % |
| Soft, ETW2, Ex compression | none | 4.246 | 4.2957 | +1.17 % |
| Hard, ETW2, Ex tension | none | 13.59 | 13.439 | −1.11 % |
| Quasi-isotropic, RTD, Ex compression | none | 7.882 | 7.8034 | −1.00 % |
| Soft, CTD, Ex compression | none | 5.125 | 5.17 | +0.88 % |
| Cross-ply UNC0, ETD1, Ex compression | none | 7.858 | 7.9269 | +0.88 % |
| Cross-ply UNC0, RTD, Ex compression | none | 7.729 | 7.7942 | +0.84 % |
| Hard, ETD1, Ex compression | none | 12.46 | 12.355 | −0.84 % |
| Hard, CTD, Ex compression | none | 12.57 | 12.657 | +0.69 % |
| Hard, CTD, Ex tension | none | 13.62 | 13.681 | +0.45 % |
| Hard, RTD, Ex tension | none | 13.14 | 13.193 | +0.41 % |
| Quasi-isotropic, ETD1, Ex compression | none | 7.878 | 7.9093 | +0.40 % |
| Hard, ETW1, Ex tension | none | 13.36 | 13.385 | +0.19 % |
| Hard, ETW2, Ex compression | none | 12.08 | 12.06 | −0.16 % |
| Cross-ply UNC0, ETW2, Ex compression | none | 7.688 | 7.699 | +0.14 % |
NCAMP, "Toray Advanced Composites TC380 T800HB 6K 2x2 Twill 200gsm with 40% RC Material Allowables Statistical Analysis Report", NCP-RP-2025-011 Rev A, September 18, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2025-023 Rev A, September 17, 2026.
Measured [Msi]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Quasi-isotropic, ETW2 modulus [Msi], Ex tension | 6.707 | 6.9592 | +3.76 % | Within 10 % |
| Soft, ETW1 modulus [Msi], Ex tension | 4.101 | 4.1931 | +2.25 % | Within 10 % |
| Quasi-isotropic, ETW1 modulus [Msi], Ex compression | 6.551 | 6.671 | +1.83 % | Within 10 % |
| Soft, ETW2 modulus [Msi], Ex tension | 3.888 | 3.9523 | +1.65 % | Within 10 % |
| Soft, RTD modulus [Msi], Ex tension | 4.334 | 4.3964 | +1.44 % | Within 10 % |
| Soft, CTD modulus [Msi], Ex compression | 4.355 | 4.3006 | −1.25 % | Within 10 % |
| Quasi-isotropic, RTD modulus [Msi], Ex tension | 7.001 | 7.0729 | +1.03 % | Within 10 % |
| Hard, CTD modulus [Msi], Ex compression | 8.5 | 8.4158 | −0.99 % | Within 10 % |
| Hard, ETW2 modulus [Msi], Ex tension | 8.999 | 9.0603 | +0.68 % | Within 10 % |
| Hard, ETW1 modulus [Msi], Ex tension | 9.04 | 9.0888 | +0.54 % | Within 10 % |
| Quasi-isotropic, CTD modulus [Msi], Ex tension | 7.326 | 7.2973 | −0.39 % | Within 10 % |
| Hard, RTD modulus [Msi], Ex tension | 8.979 | 8.995 | +0.18 % | Within 10 % |
How to reproduce it
Source
NCAMP, "Toray Advanced Composites TC380 T800HB 6K 2x2 Twill 200gsm with 40% RC Material Allowables Statistical Analysis Report", NCP-RP-2025-011 Rev A, September 18, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2025-023 Rev A, September 17, 2026.
SAR Tables 3-3 and 3-4; stacking sequences MPDR p. 21
What was taken from it
Mean measured laminate moduli in tension and compression, normalized to 0.0088 in per ply, in four environments. The report prints no laminate Poisson's ratio. CLT is built from the lamina values of the same report and environment.
Quantity compared: modulus [Msi]
Inputs
- Ply at RTD, SAR Table 3-3: tension E1 10.10 Msi, E2 9.909 Msi; compression E1 9.235 Msi, E2 9.155 Msi; ν12 0.04224, G12 0.5463 Msi
- CTD, ETW1 and ETW2 use the lamina values of their own environment from the same table
- The report prints no compression ν12, so the tension value serves the compression cases too
- Each twill ply is one orthotropic ply, so a ply printed at 45 is the ±45 ply
The inputs of each configuration are listed in the table below.
Allowed difference
10 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Quasi-isotropic, ETW2, Ex tension | none | 6.707 | 6.9592 | +3.76 % |
| Soft, ETW1, Ex tension | none | 4.101 | 4.1931 | +2.25 % |
| Quasi-isotropic, ETW1, Ex compression | none | 6.551 | 6.671 | +1.83 % |
| Soft, ETW2, Ex tension | none | 3.888 | 3.9523 | +1.65 % |
| Soft, RTD, Ex tension | none | 4.334 | 4.3964 | +1.44 % |
| Quasi-isotropic, ETW1, Ex tension | none | 6.968 | 7.0591 | +1.31 % |
| Soft, RTD, Ex compression | none | 4.083 | 4.1342 | +1.25 % |
| Soft, CTD, Ex compression | none | 4.355 | 4.3006 | −1.25 % |
| Soft, ETW1, Ex compression | none | 3.953 | 3.9984 | +1.15 % |
| Soft, CTD, Ex tension | none | 4.565 | 4.6162 | +1.12 % |
| Quasi-isotropic, RTD, Ex tension | none | 7.001 | 7.0729 | +1.03 % |
| Hard, CTD, Ex compression | none | 8.5 | 8.4158 | −0.99 % |
| Hard, CTD, Ex tension | none | 9.311 | 9.2401 | −0.76 % |
| Quasi-isotropic, ETW2, Ex compression | none | 6.49 | 6.5357 | +0.70 % |
| Hard, ETW2, Ex tension | none | 8.999 | 9.0603 | +0.68 % |
| Quasi-isotropic, RTD, Ex compression | none | 6.498 | 6.5388 | +0.63 % |
| Hard, ETW2, Ex compression | none | 8.544 | 8.4907 | −0.62 % |
| Hard, ETW1, Ex tension | none | 9.04 | 9.0888 | +0.54 % |
| Hard, ETW1, Ex compression | none | 8.524 | 8.5675 | +0.51 % |
| Quasi-isotropic, CTD, Ex tension | none | 7.326 | 7.2973 | −0.39 % |
| Hard, RTD, Ex tension | none | 8.979 | 8.995 | +0.18 % |
| Hard, RTD, Ex compression | none | 8.267 | 8.2785 | +0.14 % |
| Quasi-isotropic, CTD, Ex compression | none | 6.679 | 6.6834 | +0.066 % |
| Soft, ETW2, Ex compression | none | 3.733 | 3.7328 | −0.0067 % |
NCAMP, "Hexcel M91/IM8-GS UD Tape 145gsm with 35% RC Material Allowables Statistical Analysis Report", NCP-RP-2024-012, May 27, 2026. Stacking sequence from the Material Property Data Report CAM-RP-2025-002, June 15, 2026.
Measured [Msi]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Cross-ply UNC0, ETW modulus [Msi], Ex compression | 12.42 | 11.996 | −3.42 % | Within 10 % |
| Cross-ply UNC0, RTA modulus [Msi], Ex compression | 12.27 | 11.887 | −3.12 % | Within 10 % |
| Cross-ply UNC0, CTA modulus [Msi], Ex compression | 12.3 | 12.02 | −2.28 % | Within 10 % |
How to reproduce it
Source
NCAMP, "Hexcel M91/IM8-GS UD Tape 145gsm with 35% RC Material Allowables Statistical Analysis Report", NCP-RP-2024-012, May 27, 2026. Stacking sequence from the Material Property Data Report CAM-RP-2025-002, June 15, 2026.
SAR Table 3-3; stacking sequence MPDR p. 15
What was taken from it
Mean measured compression modulus of a [90/0]4S cross-ply, normalized to 0.0055 in per ply, in three environments. The report has no quasi-isotropic, soft or hard laminate moduli. CLT is built from the compression lamina values of the same report and environment.
Quantity compared: modulus [Msi]
Inputs
- Ply at RTA, SAR Table 3-3: compression E1 22.26 Msi, E2 1.375 Msi; ν12 0.3473; G12 0.6903 Msi
- G12 is the in-plane shear modulus from the ±45 tension test (ASTM D3518)
- The report prints only the tension ν12, so it serves the compression cases
- CTA and ETW use the lamina values of their own environment from the same table
The inputs of each configuration are listed in the table below.
Allowed difference
10 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Cross-ply UNC0, ETW, Ex compression | none | 12.42 | 11.996 | −3.42 % |
| Cross-ply UNC0, RTA, Ex compression | none | 12.27 | 11.887 | −3.12 % |
| Cross-ply UNC0, CTA, Ex compression | none | 12.3 | 12.02 | −2.28 % |
NCAMP, "Tenax-E TPWF PEEK-HTA40 E13 3K 5HS Material Allowables Statistical Analysis Report", NCP-RP-2019-004 Rev N/C, March 8, 2023. Stacking sequences from the Material Property Data Report CAM-RP-2019-007.
Measured [Msi]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Hard, RTD modulus [Msi], Ex compression | 7.055 | 7.2581 | +2.88 % | Within 10 % |
| Quasi-isotropic, ETW modulus [Msi], Ex compression | 5.703 | 5.856 | +2.68 % | Within 10 % |
| Hard, ETW modulus [Msi], Ex compression | 7.238 | 7.4113 | +2.39 % | Within 10 % |
| Quasi-isotropic, RTD modulus [Msi], Ex compression | 5.743 | 5.816 | +1.27 % | Within 10 % |
| Hard, CTD modulus [Msi], Ex tension | 7.765 | 7.833 | +0.88 % | Within 10 % |
| Soft, CTD modulus [Msi], Ex tension | 4.156 | 4.1911 | +0.84 % | Within 10 % |
| Quasi-isotropic, CTD modulus [Msi], Ex tension | 6.228 | 6.2803 | +0.84 % | Within 10 % |
| Soft, ETW modulus [Msi], Ex tension | 3.812 | 3.7922 | −0.52 % | Within 10 % |
| Soft, RTD modulus [Msi], Ex tension | 4.033 | 4.0138 | −0.48 % | Within 10 % |
How to reproduce it
Source
NCAMP, "Tenax-E TPWF PEEK-HTA40 E13 3K 5HS Material Allowables Statistical Analysis Report", NCP-RP-2019-004 Rev N/C, March 8, 2023. Stacking sequences from the Material Property Data Report CAM-RP-2019-007.
SAR Tables 3-3 and 3-4; stacking sequences MPDR Table 1-2, p. 18
What was taken from it
Mean measured laminate moduli in tension and compression, normalized to 0.01226 in per ply, in three environments. The report prints no laminate Poisson's ratio. CLT is built from the lamina values of the same report and environment.
Quantity compared: modulus [Msi]
Inputs
- Ply at RTD, SAR Table 3-3: tension E1 8.562 Msi, E2 8.435 Msi; compression E1 8.023 Msi, E2 8.070 Msi; ν12 0.03836, G12 0.5950 Msi
- CTD and ETW use the lamina values of their own environment from the same table
- The report prints no compression ν12, so the tension value serves the compression cases too
- Each 5HS ply is one orthotropic ply, so a ply printed at 45 is the ±45 ply
The inputs of each configuration are listed in the table below.
Allowed difference
10 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Hard, RTD, Ex compression | none | 7.055 | 7.2581 | +2.88 % |
| Quasi-isotropic, ETW, Ex compression | none | 5.703 | 5.856 | +2.68 % |
| Hard, ETW, Ex compression | none | 7.238 | 7.4113 | +2.39 % |
| Quasi-isotropic, RTD, Ex compression | none | 5.743 | 5.816 | +1.27 % |
| Quasi-isotropic, ETW, Ex tension | none | 5.975 | 6.0488 | +1.24 % |
| Hard, CTD, Ex tension | none | 7.765 | 7.833 | +0.88 % |
| Soft, CTD, Ex tension | none | 4.156 | 4.1911 | +0.84 % |
| Quasi-isotropic, CTD, Ex tension | none | 6.228 | 6.2803 | +0.84 % |
| Soft, ETW, Ex tension | none | 3.812 | 3.7922 | −0.52 % |
| Soft, RTD, Ex tension | none | 4.033 | 4.0138 | −0.48 % |
| Soft, RTD, Ex compression | none | 3.834 | 3.8485 | +0.38 % |
| Hard, RTD, Ex tension | none | 7.753 | 7.727 | −0.34 % |
| Hard, ETW, Ex tension | none | 7.665 | 7.6899 | +0.33 % |
| Quasi-isotropic, RTD, Ex tension | none | 6.139 | 6.1547 | +0.26 % |
| Soft, ETW, Ex compression | none | 3.703 | 3.705 | +0.053 % |
NCAMP, "Hexcel M91/IM8-GP 6K ZB Fabric PW 145gsm with 40% RC Material Allowables Statistical Analysis Report", NCP-RP-2024-011, June 2, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2025-001, June 15, 2026.
Measured [Msi]
A lab case passes at ±10 % or less. Points outside this band are known gaps, listed below with the reason.
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Quasi-isotropic, RTA modulus [Msi], Ex tension | 8.208 | 8.373 | +2.01 % | Within 10 % |
| Quasi-isotropic, CTA modulus [Msi], Ex tension | 8.363 | 8.5085 | +1.74 % | Within 10 % |
| Soft, CTA modulus [Msi], Ex tension | 5.434 | 5.5278 | +1.73 % | Within 10 % |
| Hard, RTA modulus [Msi], Ex compression | 9.542 | 9.7024 | +1.68 % | Within 10 % |
| Hard, ETW modulus [Msi], Ex compression | 9.791 | 9.9336 | +1.46 % | Within 10 % |
| Soft, RTA modulus [Msi], Ex compression | 4.956 | 4.8897 | −1.34 % | Within 10 % |
| Hard, CTA modulus [Msi], Ex tension | 10.56 | 10.695 | +1.28 % | Within 10 % |
| Soft, ETW modulus [Msi], Ex compression | 4.673 | 4.614 | −1.26 % | Within 10 % |
| Quasi-isotropic, ETW modulus [Msi], Ex tension | 8.076 | 8.1613 | +1.06 % | Within 10 % |
How to reproduce it
Source
NCAMP, "Hexcel M91/IM8-GP 6K ZB Fabric PW 145gsm with 40% RC Material Allowables Statistical Analysis Report", NCP-RP-2024-011, June 2, 2026. Stacking sequences from the Material Property Data Report CAM-RP-2025-001, June 15, 2026.
SAR Tables 3-6 and 3-9; stacking sequences MPDR Table 1-2, p. 20
What was taken from it
Mean measured laminate moduli in tension and compression, normalized to 0.0061 in per ply, in three environments. The report prints no laminate Poisson's ratio. CLT is built from the lamina values of the same report and environment.
Quantity compared: modulus [Msi]
Inputs
- Ply at RTA, SAR Table 3-6: tension E1 11.72 Msi, E2 11.93 Msi; compression E1 10.76 Msi, E2 10.78 Msi; ν12 0.04125, G12 0.6602 Msi
- G12 is the in-plane shear modulus from the ±45 tension test (ASTM D3518), not the V-notched rail shear value the report also prints
- CTA and ETW use the lamina values of their own environment from the same table
- The hard tension and compression specimens have different stacking sequences, and each case uses its own
- Each plain weave ply is one orthotropic ply, and the tension ν12 serves the compression cases too
The inputs of each configuration are listed in the table below.
Allowed difference
10 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Quasi-isotropic, RTA, Ex tension | none | 8.208 | 8.373 | +2.01 % |
| Quasi-isotropic, CTA, Ex tension | none | 8.363 | 8.5085 | +1.74 % |
| Soft, CTA, Ex tension | none | 5.434 | 5.5278 | +1.73 % |
| Hard, RTA, Ex compression | none | 9.542 | 9.7024 | +1.68 % |
| Hard, ETW, Ex compression | none | 9.791 | 9.9336 | +1.46 % |
| Soft, RTA, Ex compression | none | 4.956 | 4.8897 | −1.34 % |
| Hard, CTA, Ex tension | none | 10.56 | 10.695 | +1.28 % |
| Soft, ETW, Ex compression | none | 4.673 | 4.614 | −1.26 % |
| Hard, RTA, Ex tension | none | 10.51 | 10.636 | +1.20 % |
| Hard, ETW, Ex tension | none | 10.41 | 10.523 | +1.08 % |
| Quasi-isotropic, RTA, Ex compression | none | 7.597 | 7.6777 | +1.06 % |
| Quasi-isotropic, ETW, Ex tension | none | 8.076 | 8.1613 | +1.06 % |
| Quasi-isotropic, ETW, Ex compression | none | 7.643 | 7.7217 | +1.03 % |
| Soft, ETW, Ex tension | none | 4.811 | 4.8342 | +0.48 % |
| Soft, RTA, Ex tension | none | 5.224 | 5.2406 | +0.32 % |
Albert, C. & Fernlund, G., "Spring-in and Warpage of Angled Composite Laminates", Compos Sci Technol 62 (2002) 1895-1912.
Largest error against the reference for each configuration, worst first. The axis is logarithmic: each step up is ten times the error.
4 configurations, largest error first
Cases, largest error first
| Case | Reference | Ours | Error | Status |
|---|---|---|---|---|
| Albert & Fernlund [0]n angle, included 90° spring-in Δθ [°], Δθ_CTE | 0.58 | 0.58737 | +1.27 % | Over 1 % |
| Albert & Fernlund [0]n angle, included 135° spring-in Δθ [°], Δθ_CTE | 0.29 | 0.29369 | +1.27 % | Over 1 % |
| Albert & Fernlund QI angle, included 90° spring-in Δθ [°], Δθ_CS | 0.46 | 0.46504 | +1.09 % | Over 1 % |
| Albert & Fernlund QI angle, included 135° spring-in Δθ [°], Δθ_CS | 0.23 | 0.23252 | +1.09 % | Over 1 % |
How to reproduce it
Source
Albert, C. & Fernlund, G., "Spring-in and Warpage of Angled Composite Laminates", Compos Sci Technol 62 (2002) 1895-1912.
Table 1, p. 1897
What was taken from it
The published spring-in predictions of the Radford model in Table 1.
Quantity compared: spring-in Δθ [°]
Inputs
The inputs of each configuration are listed in the table below.
Allowed difference
per sub-case, below; 2 %
Compared values, largest error first
| Value | Layup | Reference | Ours | Error |
|---|---|---|---|---|
| Albert & Fernlund [0]n angle, included 90°, Δθ_CTE | unidirectional | 0.58 | 0.58737 | +1.27 % |
| Albert & Fernlund [0]n angle, included 135°, Δθ_CTE | unidirectional | 0.29 | 0.29369 | +1.27 % |
| Albert & Fernlund QI angle, included 90°, Δθ_CS | quasi-isotropic | 0.46 | 0.46504 | +1.09 % |
| Albert & Fernlund QI angle, included 135°, Δθ_CS | quasi-isotropic | 0.23 | 0.23252 | +1.09 % |
| Albert & Fernlund QI angle, included 90°, Δθ | quasi-isotropic | 1.28 | 1.2933 | +1.04 % |
| Albert & Fernlund QI angle, included 135°, Δθ | quasi-isotropic | 0.64 | 0.64664 | +1.04 % |
| Albert & Fernlund QI angle, included 90°, Δθ_CTE | quasi-isotropic | 0.82 | 0.82825 | +1.01 % |
| Albert & Fernlund QI angle, included 135°, Δθ_CTE | quasi-isotropic | 0.41 | 0.41413 | +1.01 % |
The tick on each bar marks the limit for that group. A bar past the tick is over the limit.
How the numbers are checked
The two groups answer two different questions. Reference solutions check that the program solves its equations correctly: the same model, solved by someone else in a published solution, an independent implementation or a finite element model, gives the same number. Engineers call this verification. Lab tests check that the equations describe a real part, which no amount of matching other programs can show. That is validation. A method can pass every verification case and still differ from a test, because the model leaves something out. The terms follow NAFEMS, What is Verification and Validation? (2014).
A reference case counts as within when its error is at most 1 %, a lab case when it is at most 10 %. A known gap is a case where the method and the reference disagree for a reason that is understood. It stays on this page with its reason until the method changes.