Hashin Failure Criterion

The Hashin failure criterion for a composite ply: its four failure modes, the formulas, the safety factor, and one ply worked by hand.

Try it live: Failure Criteria Calculator
Opens with the +45° ply from the worked example below. Change a stress and the Hashin mode updates.
Open live calculator →

What the Hashin criterion predicts

Hashin splits ply failure into four mechanisms: fiber tension, fiber compression, matrix tension and matrix compression1. Each mode has its own failure index, and the sign of σ1 and σ2 decides which fiber mode and which matrix mode apply. The larger of the two indices governs. So besides a number, Hashin tells you how the ply fails: fibers breaking, or the matrix cracking between them.

It assumes a homogeneous orthotropic ply in plane stress, loaded linearly to failure.

Hashin belongs to the failure-mode family. The cards draw each family's failure envelope for the same ply in the σ1-σ2 plane, with no shear.

σ1σ2
No interaction
Max stressMax strain

Each stress, or each strain, is checked against its own limit. Max stress draws a box with sharp corners. Max strain draws a slanted box, because the Poisson effect puts some σ1 into ε2.

σ1σ2
Quadratic interaction
Tsai-HillTsai-Wu

All stresses go into one quadratic expression. The envelope is one smooth, ellipse-like curve, and it does not say whether the fiber or the matrix failed.

σ1σ2
Failure modes
HashinPuck

Fiber and matrix failure get separate checks. The envelope is pieced together from one curve or line per mode.

Also in this family, not drawn: Cuntze, Sun, Edge.

When to use Hashin

Use it when the failure mode matters. Matrix cracking in one ply is often survivable, while fiber failure usually ends the laminate, so the mode changes what you do next. Hashin is also the usual damage initiation check in progressive failure analysis, which degrades a ply differently per mode. For a single interaction index without a mode, use Tsai-Wu. When the matrix is in transverse compression, use Puck, or Cuntze with fewer parameters. Edge also names one mode per ply and links shear with fiber compression.

Hashin formula

Four failure modes:

Fiber tension (σ1≥0):\text{Fiber tension } (\sigma_1 \ge 0):
(σ1S1t)2+(τ12S12)2≥1\left(\frac{\sigma_1}{S_{1t}}\right)^2 + \left(\frac{\tau_{12}}{S_{12}}\right)^2 \ge 1
Fiber compression (σ1<0):\text{Fiber compression } (\sigma_1 < 0):
(−σ1S1c)2≥1\left(\frac{-\sigma_1}{S_{1c}}\right)^2 \ge 1
Matrix tension (σ2≥0):\text{Matrix tension } (\sigma_2 \ge 0):
(σ2S2t)2+(τ12S12)2≥1\left(\frac{\sigma_2}{S_{2t}}\right)^2 + \left(\frac{\tau_{12}}{S_{12}}\right)^2 \ge 1
Matrix compression (σ2<0):(σ22ST)2+[(S2c2ST)2−1]σ2S2c+(τ12S12)2≥1\text{Matrix compression } (\sigma_2 < 0): \quad \left(\frac{\sigma_2}{2S_T}\right)^2 + \left[\left(\frac{S_{2c}}{2S_T}\right)^2 - 1\right]\frac{\sigma_2}{S_{2c}} + \left(\frac{\tau_{12}}{S_{12}}\right)^2 \ge 1

where ST=S2c/2S_T = S_{2c}/2 (transverse shear strength approximation). Failure when any mode index reaches 1.0.

ST is the transverse shear strength, the shear strength on a plane through the thickness parallel to the fibers. Coupon tests rarely give it, so the calculator and the dashboard set ST = S2c/2. With that choice the bracketed term is zero, and matrix compression reduces to (σ2/S2c)2 + (τ12/S12)2.

Failure index and safety factor

The failure index is the larger of the active fiber index and the active matrix index. Each mode index is quadratic in stress, so the calculator gives the safety factor as SF = 1/√FI2. The overview covers safety factors and margins for all criteria.

Worked example: one ply

Take the +45° ply of the quasi-isotropic laminate example, T300/5208 carbon/epoxy. Its stresses are σ1 = −93.31 MPa, σ2 = −6.69 MPa and τ12 = −40.01 MPa. Both normal stresses are compressive, so the fiber compression and matrix compression modes apply, with S1c = 1500 MPa, S2c = 246 MPa and S12 = 68 MPa.

Fiber compression: (σ1/S1c)20.00387
Matrix compression: (σ2/S2c)20.0007396
Matrix compression: (τ12/S12)20.3462
Matrix compression index0.3469

Matrix compression governs, and almost all of it is shear. FI = 0.3469 and SF = 1/√FI = 1.698. The ply would crack in the matrix long before the fibers are in danger.

Limitations

  • Fiber compression is a maximum stress check with no shear interaction. For a better compression prediction, consider Puck.
  • ST is rarely measured. The S2c/2 estimate sets the matrix compression result.
  • It predicts first-ply failure only. Damage after that is covered on progressive failure.

Frequently asked questions

Fiber tension, fiber compression, matrix tension and matrix compression. The sign of σ1 picks the fiber mode and the sign of σ2 picks the matrix mode.

References

  1. Hashin, Z., "Failure Criteria for Unidirectional Fiber Composites", J. Applied Mechanics, Vol. 47, 1980, pp. 329-334. doi:10.1115/1.3153664
  2. Tsai, S.W. & Hahn, H.T., Introduction to Composite Materials, Technomic, 1980.
Written by Rick Schrijver