Tsai-Wu Failure Criterion
The Tsai-Wu failure index for a composite ply: the formula, the strength coefficients, how the safety factor follows from it, and one ply worked by hand.
What the Tsai-Wu criterion predicts
Tsai-Wu folds the three in-plane ply stresses, σ1 along the fibers, σ2 across them and the shear τ12, into one failure index (FI). The ply fails when FI reaches 11,2. It is a tensor polynomial with linear and quadratic terms, and the linear terms are what set it apart: they let a ply be stronger in compression than in tension. The carbon/epoxy in the worked example below is about six times stronger in compression than in tension across the fibers (246 against 40 MPa).
The criterion assumes a homogeneous orthotropic ply in plane stress, loaded linearly up to failure. It returns a number, not a mechanism. It does not say whether fibers or matrix gave way.
Tsai-Wu belongs to the quadratic interaction family. The cards draw each family's failure envelope for the same ply in the σ1-σ2 plane, with no shear.
Each stress, or each strain, is checked against its own limit. Max stress draws a box with sharp corners. Max strain draws a slanted box, because the Poisson effect puts some σ1 into ε2.
All stresses go into one quadratic expression. The envelope is one smooth, ellipse-like curve, and it does not say whether the fiber or the matrix failed.
Fiber and matrix failure get separate checks. The envelope is pieced together from one curve or line per mode.
Also in this family, not drawn: Cuntze, Sun, Edge.
When to use Tsai-Wu
Use it for general first-ply failure checks under combined loading, and whenever the tensile and compressive strengths of the ply differ. That covers most fiber-reinforced plastics. When you need the failure mode, for damage modeling or for a report that says "matrix cracking", use Hashin next to it. When the tensile and compressive strengths are close, Tsai-Hill gives nearly the same answer with fewer inputs. For a first check with no interaction, use max stress, or max strain when your allowables are strains.
Tsai-Wu formula
In plane stress the failure index is2:
with the strength coefficients
Failure when FI ≥ 1.0
S1t and S1c are the tensile and compressive strengths along the fibers, S2t and S2c across them, and S12 the in-plane shear strength, all entered as positive numbers. The interaction coefficient F12 would need a biaxial test to measure. The value above, F12 = −½√(F11F22), is the usual estimate3, and it is the one the calculator and the dashboard use.
Failure index and safety factor
Because of the linear terms, the Tsai-Wu index does not scale with the load. Double every stress and the quadratic part Q grows four times while the linear part L only doubles. So the safety factor is not 1/FI. It is the factor R that brings the scaled stresses onto the failure surface:
L = F1σ1 + F2σ2 and Q is the rest of the polynomial, so FI = L + Q. R above 1 means the ply holds, and R is the factor the load can still grow by. The overview covers safety factors and margins for all criteria.
Worked example: one ply
Take the +45° ply of the quasi-isotropic laminate example. It is T300/5208 carbon/epoxy, with S1t = S1c = 1500 MPa, S2t = 40 MPa, S2c = 246 MPa and S12 = 68 MPa. Its stresses are σ1 = −93.31 MPa, σ2 = −6.69 MPa and τ12 = −40.01 MPa.
| F1σ1 | 0 |
| F2σ2 | −0.1401 |
| F11σ12 | 0.00387 |
| F22σ22 | 0.004548 |
| F66τ122 | 0.3462 |
| 2F12σ1σ2 | −0.004195 |
F1 is zero because S1t = S1c. The F2σ2 term is negative: the ply is squeezed across the fibers, and Tsai-Wu counts that as a credit. Shear makes up almost all of Q. The sum is FI = 0.2104, and the safety factor from the quadratic is R = 1.901. Note that 1/FI would give 4.754, which is wrong for this criterion.
Limitations
- One index, no failure mode. The dashboard estimates the dominant mode from stress ratios, but a mode-based criterion such as Hashin or Puck gives the mechanism.
- F12 is an estimate unless you have biaxial test data, and the predicted strength under biaxial stress depends on it1.
- The linear F2σ2 term means transverse compression raises the allowed shear. In the worked example that changes which ply fails first compared with Tsai-Hill.
- It predicts first-ply failure only. What the laminate carries after that is a progressive failure question.
Frequently asked questions
References
- Jones, R.M., Mechanics of Composite Materials, 2nd Ed., Taylor & Francis, 1999.
- Tsai, S.W. & Wu, E.M., "A General Theory of Strength for Anisotropic Materials", J. Composite Materials, Vol. 5, 1971. doi:10.1177/002199837100500106
- Tsai, S.W. & Hahn, H.T., Introduction to Composite Materials, Technomic, 1980.